Nitric Acid Alloy Selection: 304L NAG vs 310L vs Alloy 20 (58 chars)
Date: 2025年10月2日 Categories: News Views: 376
By Shanghai Hangbo Alloy Group Co., Ltd. - China Supplier | ISO 9001:2015 | Est. 2012
Contact: sales@hangboalloy.com | hangbo@nickel-alloy.com | WhatsApp (Lisa): +86 13611656360
Quick Answer: Which Alloy Should You Use for Nitric Acid?
Use 304L nitric acid grade for dilute to 65% nitric acid at low to moderate temperature, 310L or a high-silicon austenitic where the same acid runs hot or concentrated, Alloy 20 or 825 where chlorides or sulphuric acid are also present, and titanium for chloride-bearing nitric duties below the fuming range. Fuming acid above 98% needs aluminium or a high-silicon grade, never 304L.
Key Takeaways
- Nitric acid is oxidising, so cheap chromium-rich grades beat expensive molybdenum-rich ones. The passive film is self-healing in nitric acid; C-276 and other high-molybdenum grades are usually the wrong answer and cost three to five times more.
- The purchase specification for 304L NAG is a corrosion rate, not a chemistry. Restricted carbon, silicon, phosphorus and sulphur exist only to pass the Huey test, ASTM A262 Practice C, and the test result is the acceptance criterion.
- Chromium sets the ceiling. 18% Cr serves dilute acid at ambient temperature, 25% Cr (310L) serves the azeotrope at moderate temperature, and high-silicon austenitics serve hot concentrated and fuming conditions.
- Chloride is the impurity that decides most real failures. 50-100 ppm chloride is enough to pit and crack 304L in hot nitric acid, and it is the single most common reason a nitric plant pays for Alloy 20 or 825 instead of 304L.
- The condenser is the hardest duty in the plant. The first condensing zone combines hot vapour, concentrated liquid, non-condensables and chloride concentration, so tube grade and velocity must be selected for that zone, not for the bulk acid.
- Welds and free iron fail before the parent metal does. Low-carbon welding practice, Mo-free filler, ASTM A380 cleaning and a Huey test on the weld procedure are what separate a 15-year nitric circuit from a three-year one.
Why Oxidising Nitric Acid Inverts the Usual Alloy Rules
Nitric acid is a strongly oxidising acid, and an oxidising acid stabilises the chromium oxide film on stainless steel instead of stripping it. That single electrochemical difference is why the alloy ranking for nitric service looks almost exactly inverted compared with hydrochloric or dilute sulphuric acid service: chromium content dominates, molybdenum contributes little or nothing, and the premium nickel alloys are usually unnecessary. In nitric acid the cathodic reaction is nitrate reduction, which holds the steel potential well above the passivation potential, so a grade with enough chromium stays passive even in quite aggressive acid.
The practical consequence is that a 304L nitric acid grade plate costing a few dollars per kilogram outperforms C-276 in 65% nitric acid at 60 °C, and does so for decades. Molybdenum, which is the workhorse addition in reducing acid service, forms MoO3 in strongly oxidising nitric acid; the oxide is volatile at elevated temperature and the enrichment of molybdenum in the passive film is not the benefit it is in hydrochloric acid. This is why nitric plant specifications that were copied from a hydrochloric plant fail on the first inspection: C-276 is not a nitric acid alloy, and paying for it buys no corrosion resistance while adding cost, delivery risk and welding complexity.
The same logic explains why copper-bearing grades are not automatically disqualified. Alloy 20 and 825 both carry copper, which is there for sulphuric acid resistance, and 2-3.5% molybdenum, which is there for the same reason. In pure nitric acid those additions are neutral to slightly negative; in nitrating mixed acid, where sulphuric acid is present in large excess, they are essential and dominate the decision. The selection question is therefore never "what is the best alloy for nitric acid" but "what else is in the stream".
| Alloying element | Effect in oxidising nitric acid | Effect in reducing acid | Practical selection meaning |
|---|---|---|---|
| Chromium, 18% | Stable passive film to roughly 65% acid at moderate temperature (typical) | Film unstable without oxidiser | Minimum for dilute ambient nitric service |
| Chromium, 25-26% | Extends passive range to hot azeotropic acid (typical) | Moderate benefit | Basis of 310L and high-silicon grades |
| Molybdenum, 2-4% | Neutral at low temperature, can raise corrosion rate at high temperature and concentration (typical) | Strong benefit, prevents active dissolution | Useful only when sulphuric acid or chloride is present |
| Silicon, 4-6% | Strong benefit in hot concentrated and fuming nitric acid (typical) | Limited benefit | Basis of high-silicon austenitic grades |
| Nickel, 20-40% | Stabilises austenite, allows high chromium without sigma | Beneficial in reducing acids | Required for hot concentrated service |
| Copper, 1-4% | Neutral to slightly negative in pure nitric acid | Strong benefit in sulphuric acid | Justified by mixed acid, not by nitric acid alone |
| Carbon, under 0.020% | Prevents chromium carbide precipitation at grain boundaries | Same | Mandatory for welded nitric equipment |
| Titanium addition (stabilisation) | No benefit in nitric, added for intergranular control after welding | Same | Not a substitute for low carbon in NAG grades |
Table note: qualitative directions summarised from ASTM G31 immersion-test practice and from ASTM A262 Practice C acceptance experience in nitric plant service; individual values are typical and must be confirmed against the specific concentration, temperature and chloride level.
304L Nitric Acid Grade: The Huey Test Is the Purchase Specification
Nitric acid grade 304L is not simply low-carbon 304L with a different label. It is a grade in which carbon, silicon, phosphorus and sulphur are restricted beyond the standard analysis, and the restrictions exist only to control intergranular attack in boiling nitric acid. Buying it on chemistry alone misses the point: two heats can both meet a restricted chemistry table and still differ by a factor of five in measured corrosion rate, because the sensitisation behaviour of the heat, its inclusion content and its grain size all feed into the result. The number that matters is the corrosion rate from ASTM A262 Practice C, and that number belongs in the purchase order.
Practice C, the Huey test, exposes a sensitised specimen to boiling 65% nitric acid for five consecutive 48-hour periods, with the specimen weighed after each period and the solution renewed. The test is severe precisely because nitric acid is oxidising: any chromium-depleted zone at a grain boundary is attacked at a rate that a sulphuric acid test would not resolve. The usual acceptance criterion for 304L nitric acid grade is a maximum of about 0.6 mm/y (0.024 in/y) in each of the five periods, and many nitric acid and adipic acid specifications tighten the five-period average to roughly 0.36 mm/y (0.014 in/y). Both figures are typical buyer requirements rather than values written into ASTM A262, so the drawing or purchase order must state which rule applies and whether a single failed period rejects the lot.
The chemistry restrictions make sense against that test. Carbon is held to about 0.020% or below to keep chromium carbides out of solution during welding and any subsequent slow cooling; silicon is restricted because silicon-rich phases and slag inclusions act as initiation sites in the boiling acid; phosphorus and sulphur are restricted because phosphide and sulphide inclusions dissolve preferentially and leave pits that the Huey test detects as mass loss. Mills that routinely roll nitric acid grade keep separate consumable practice for it, and the mill certificate should show the restricted values as measured, not as "typical of grade".
There is a second, equally important consequence: the weld is the part of a nitric acid vessel that fails. A parent plate that passes Practice C at 0.2 mm/y can produce a weld Heat Affected Zone at 1.0 mm/y if the heat input and interpass temperature are not controlled, because the weld thermal cycle re-creates the chromium-depleted boundary that the low-carbon chemistry was bought to avoid. Weld procedure qualification for nitric service therefore has to include corrosion testing of a production-representative welded coupon, not just tensile and bend tests. This is where most Chinese-supplied nitric acid equipment either earns its service life or loses it, and it is a documentation issue as much as a metallurgical one.
| Element | Standard 304L per ASTM A240 | 304L nitric acid grade, typical purchase limits | Reason for the restriction |
|---|---|---|---|
| Carbon | 0.030 max | 0.020 max | Avoid chromium carbide precipitation and sensitisation |
| Silicon | 0.75 max | 0.30 max | Reduce inclusion-initiated attack in boiling acid |
| Phosphorus | 0.045 max | 0.020 max | Limit phosphide inclusions that dissolve preferentially |
| Sulphur | 0.030 max | 0.005 max | Limit sulphide inclusions and improve weld cleanliness |
| Chromium | 18.0-20.0 | 18.0-20.0 | Passive film former, unchanged |
| Nickel | 8.0-12.0 | 9.0-12.0 | Austenite stability, slightly narrowed |
| Molybdenum | 0.75 max (residual) | 0.30 max | Residual Mo avoided in strongly oxidising acid |
| Huey test, ASTM A262 Practice C | Not required | Max 0.6 mm/y per period, typical | Direct measure of intergranular resistance |
| Intergranular screening | Not required | Practice A etch plus Practice C, typical | Reject sensitised heats before fabrication |
Table note: base chemistry limits per ASTM A240 / ASTM A480 (latest edition); the nitric acid grade column contains typical mill and buyer limits, not standard limits, and must be confirmed on the mill certificate and in the purchase order.
The Concentration and Temperature Map, Including the Fuming Range
Nitric acid changes character three times between 0% and 100%, and each change moves the grade choice. Dilute acid below about 30% is a moderately oxidising aqueous acid that 304L handles at ambient and slightly elevated temperature; the 65-68% azeotrope is a strongly oxidising acid that needs 25% chromium once it boils; and acid above 98%, which contains dissolved NO2 and is described as fuming, is a different chemical system in which neither 304L nor any standard austenitic should be used. Temperature moves each boundary downward, and the practical selection table is therefore two-dimensional.
At the dilute end, the counter-intuitive fact is that carbon steel is the wrong material and 304L is the right one. Cold dilute nitric acid attacks carbon steel at a rate that makes a storage tank a maintenance item, while the same steel in 65-70% acid at ambient passivates and has been used for concentrated acid storage for a century. The inversion is worth stating explicitly in a specification review, because a reviewer who knows that "carbon steel is fine for nitric" from a concentrated acid plant will otherwise apply the rule to a 20% scrubber liquor and be surprised by the result.
Between 30% and 68%, chromium content separates the grades. 304L NAG is comfortable in 40-60% acid at temperatures up to roughly 40-50 °C, and its corrosion rate rises steeply as the boiling point is approached. 310L, with 24-26% chromium and 19-22% nickel, holds its passive film in boiling 65% acid and is the standard choice for azeotropic duty, reboilers and hot acid piping. High-silicon austenitics, with 3.7-4.5% silicon and about 18% chromium, extend the range further into hot concentrated acid and are used where 310L shows unacceptable metal loss or where the acid is contaminated with oxidising species that raise the potential.
Above 98%, the fuming range, the correct materials are aluminium and high-silicon austenitic grades, with 310L acceptable only in specific low-temperature situations. Fuming nitric acid contains free NO2, has very low water activity and attacks austenitic stainless steels intergranularly at rates that can exceed 1 mm/y within a single campaign. Aluminium 1060 has been the standard material for fuming acid storage and rail transport for decades because it forms a stable aluminium oxide film in the near-anhydrous acid. The engineering caution is that aluminium is a low-strength material with a low melting point, so it is used for tanks and lines rather than for heat exchanger tubes, and it must never be specified for dilute acid, which dissolves it.
| Acid concentration | Temperature | First choice | Alternative | Typical corrosion rate of the first choice | Governing risk |
|---|---|---|---|---|---|
| Below 30% | Ambient to 40 °C | 304L NAG | 304L standard, 316L | Under 0.1 mm/y | Chloride pitting, aeration effects |
| Below 30% | 40-80 °C | 304L NAG | 310L, 904L | 0.1-0.3 mm/y | Chloride SCC, velocity |
| 30-65% | Ambient to 50 °C | 304L NAG | 310L | 0.1-0.5 mm/y | Intergranular attack at welds |
| 30-65% | 50-100 °C | 310L | High-silicon austenitic | 0.1-0.5 mm/y | Sensitisation, weld decay |
| 65-68% azeotrope | Boiling, about 120 °C | 310L | High-silicon austenitic, titanium below 65% | 0.3-0.8 mm/y | Intergranular corrosion, NOx |
| 68-98% | Ambient to 40 °C | 310L, high-silicon austenitic | Titanium only with strict water control | 0.1-0.5 mm/y | Intergranular attack, velocity |
| Above 98% fuming, NO2 present | Ambient to 30 °C | Aluminium 1060 | High-silicon austenitic | Under 0.1 mm/y for aluminium | Vigorous attack on stainless, NO2 reaction |
| Nitrating mixed acid, HNO3 plus H2SO4 | 30-90 °C | 304L NAG | Alloy 20, 825 | 0.1-0.4 mm/y | Sulphate reducing character, chlorides |
Table note: concentration and temperature bands describe typical plant practice and typical corrosion rates from ASTM G31 immersion testing; 304L values assume nitric acid grade material meeting ASTM A262 Practice C. Confirm every selection against the actual stream analysis.
Chloride Is the Hidden Impurity That Decides Most Nitric Acid Failures
Chloride at 50-100 ppm is enough to convert a comfortable 304L nitric acid duty into a pitting and stress corrosion cracking problem, and it is the impurity most often missing from the data sheet. The mechanism is a potential problem rather than an acid problem: nitric acid holds the steel at a high potential, close to the pitting breakdown potential, so the chloride threshold for pitting in nitric acid is much lower than in neutral water or in dilute sulphuric acid. A nitric acid circuit that is clean at 10 ppm chloride has a wide margin; the same circuit at 80 ppm in a hot zone, with a deposit or a weld scale to act as a crevice, does not.
The sources are mundane and almost always process-side rather than material-side. Cooling water leaking into a condenser, raw material contaminated with salt, catalyst residues, chlorinated additives in a nitration reaction, and wash water from a neighbouring chlorinated circuit all introduce chloride. The concentration step is the dangerous part: an evaporator, a reboiler or a condenser concentrates non-volatile chloride in the liquid film, so a bulk analysis of 20 ppm can correspond to several hundred ppm in the condensate that wets the tube wall. Sampling the bulk acid and concluding the stream is chloride-free is one of the most common errors in nitric acid materials selection.
Stress corrosion cracking follows pitting and is the failure mode that ends campaigns abruptly. Austenitic stainless steels crack in chloride-bearing nitric acid above roughly 60 °C, and the cracking is transgranular, fast, and usually initiates at a weld toe, a U-bend in a tube or a region of cold work. Cold work is a genuine accelerator: a rolled tube end or a bent line that would be acceptable in the annealed condition can crack in weeks when it carries residual tensile stress in a hot chloride-bearing acid. That is why nitric acid piping specifications frequently require solution annealing after bending and why tube expansion practice matters as much as tube grade.
Once chlorides are confirmed, the response is a step up in chromium and, usually, in molybdenum and nickel. 310L improves pitting resistance through chromium alone and is the cheapest step. 904L adds 4-5% molybdenum and 1.5% copper and is the standard answer for nitric acid with a few hundred ppm chloride at moderate temperature. Alloy 20 and 825 add more nickel and are used where chloride coexists with sulphuric acid. Titanium is effectively immune to chloride pitting and chloride SCC in nitric acid, which is why titanium condenser tubing appears in nitric plants with brackish cooling water, but titanium has its own limits in the fuming range described below.
| Chloride level in the acid | Temperature | 304L NAG | 310L | 904L | Alloy 20 / 825 | Ti Gr2 |
|---|---|---|---|---|---|---|
| Under 20 ppm | Under 60 °C | Suitable | Suitable | Suitable | Suitable | Suitable |
| 20-50 ppm | Under 60 °C | Suitable, monitor | Suitable | Suitable | Suitable | Suitable |
| 50-100 ppm | 60-90 °C | Not recommended | Marginal, typical | Suitable | Suitable | Suitable |
| 100-500 ppm | 60-90 °C | Not suitable | Not recommended | Marginal, typical | Suitable | Suitable |
| 500-1000 ppm | Under 60 °C | Not suitable | Not suitable | Not recommended | Suitable | Suitable |
| Above 1000 ppm, any temperature | Any | Not suitable | Not suitable | Not suitable | Marginal, verify by test | Suitable below fuming range |
Table note: thresholds are typical engineering judgements based on ASTM G48 pitting-test practice and ASTM G31 immersion experience in nitric acid; they are not standard limits and shift with temperature, velocity, surface finish and crevice geometry.
Alloy 20, 825 and 904L: Mixed Acid, Chloride and the Economic Middle
Alloy 20 and 825 are not primarily nitric acid alloys, and specifying them for pure nitric acid is usually a waste of money; they earn their place when nitric acid is mixed with sulphuric acid or carries chloride. Nitrating mixed acid is exactly that case. A nitration stream typically contains 15-30% nitric acid with 50-70% sulphuric acid, plus dissolved NOx and often chloride from chlorinated feedstock, and that mixture behaves as a reducing-to-mixed acid in which molybdenum and copper are beneficial rather than neutral. This is the classic Alloy 20 application, and it is where the grade's niobium stabilisation and 3-4% copper pay for themselves.
Alloy 20 (N08020) contains 19-21% chromium, 32-38% nickel, 2-3% molybdenum, 3-4% copper and niobium plus tantalum at eight times the carbon content. The niobium stabilisation is what allows it to be welded without sensitisation in mixed acid, and its copper content gives it resistance to sulphuric acid that 904L cannot match at the same cost. Its nitric acid resistance is good but not exceptional: in boiling 65% nitric acid its Huey rate is typically higher than a properly produced 304L NAG, which is why it is not the grade to choose for a nitric acid storage tank or a nitric acid fractionator. It is the grade to choose for the nitrator, the mixed acid feed line and the spent acid recovery section.
Incoloy 825 (N08825) sits above Alloy 20 in nickel, at 38-46%, with 19.5-23.5% chromium, 2.5-3.5% molybdenum, 1.5-3% copper and a titanium addition. The higher nickel improves resistance in hot sulphuric acid and reduces the tendency to chloride SCC, and the titanium stabilisation controls intergranular attack after welding. In nitric acid plants 825 appears in mixed acid coolers, spent acid concentrators and in nitric acid duties that carry several hundred ppm chloride at 80-100 °C, where 904L is marginal and Alloy 20 does not have the nickel to hold up. It is not a fuming acid material and it is not a substitute for 310L at the azeotrope.
904L (N08904) is the grade engineers reach for when the word "chloride" appears, and it is a reasonable middle option for nitric acid containing a few hundred ppm chloride at moderate temperature. Its 4-5% molybdenum and 1.5% copper give it pitting resistance far above 310L, and its 20-23% chromium keeps it passive in oxidising acid. What 904L does not do is tolerate strongly oxidising nitric acid at high temperature, where its molybdenum content is not an advantage and its corrosion rate can exceed that of a plain high-chromium grade. Treat 904L as a chloride solution rather than as a nitric acid upgrade, and confirm the choice with immersion testing when the acid is above 65% and hot.
| Grade | UNS | Standard | C max | Cr | Ni | Mo | Cu | Other | Typical nitric role |
|---|---|---|---|---|---|---|---|---|---|
| 304L NAG | S30403 | ASTM A240 / A480 | 0.020 | 18.0-20.0 | 9.0-12.0 | 0.30 max | - | Si 0.30 max, P 0.020 max, S 0.005 max | Dilute to 65% acid, ambient to moderate temperature |
| 310L / 310S | S31003 / S31008 | ASTM A240 / A480 | 0.030 / 0.08 | 24.0-26.0 | 19.0-22.0 | 0.75 max | - | - | Hot azeotropic acid, reboilers, hot acid piping |
| High-silicon austenitic | S30600 | Mill specification, EN 1.4361 | 0.020 | 17.0-18.5 | 14.0-15.5 | 0.5 max | - | Si 3.7-4.5 | Hot concentrated and fuming acid, nitric acid catalyst handling |
| Alloy 20 | N08020 | ASTM B463 / B464 / B468 | 0.07 | 19.0-21.0 | 32.0-38.0 | 2.0-3.0 | 3.0-4.0 | Nb+Ta 8xC min | Nitrating mixed acid, spent acid recovery |
| 825 | N08825 | ASTM B423 / B424 / B425 | 0.05 | 19.5-23.5 | 38.0-46.0 | 2.5-3.5 | 1.5-3.0 | Ti 0.6-1.2 | Mixed acid with chloride, hot spent acid |
| 904L | N08904 | ASTM B673 / B674 / B677 | 0.020 | 19.0-23.0 | 23.0-28.0 | 4.0-5.0 | 1.0-2.0 | - | Nitric acid with 100-500 ppm chloride, moderate temperature |
| Titanium Gr2 | R50400 | ASTM B265 / B338 | 0.08 max (O 0.25 max) | - | - | - | - | Ti balance, Fe 0.30 max | Condenser tubes, chloride-bearing nitric acid below fuming range |
Table note: composition limits per ASTM A240 / ASTM A480, ASTM B463, ASTM B424, ASTM B673 and ASTM B265 (latest editions); the 304L nitric acid grade restrictions and the high-silicon grade range are typical mill limits rather than standard limits.
The cross-reference table below is the one to use when a drawing arrives with a European designation, a Chinese GB grade or a Russian grade and the mill needs to roll to a UNS number. Note where no direct equivalent exists, because a "closest" grade is not a substitute in nitric acid service: silicon and carbon limits that differ by a few hundredths of a percent are exactly what the Huey test detects.
| Grade | UNS | ASTM product specs | EN / DIN | GB (China) | GOST (Russia) | Notes |
|---|---|---|---|---|---|---|
| 304L | S30403 | A240, A312, A213 | 1.4306 / 1.4307 | 022Cr19Ni10 | 03Kh18N11 | NAG variant is a purchase specification, not a separate UNS |
| 310S / 310L | S31008 / S31003 | A240, A312, A213 | 1.4845 / 1.4841 | 06Cr25Ni20 | 20Kh23N18 | 310L is often dual-certified with 310S |
| High-silicon austenitic | S30600 | Mill specification | 1.4361 | Not standardised | Not standardised | Confirm silicon range and Huey result on each heat |
| Alloy 20 | N08020 | B463, B464, B468, B473 | 2.4660 | NS1403 | 06KhN28MDT (closest) | Niobium stabilised, copper bearing |
| 825 | N08825 | B423, B424, B425, B163 | 2.4858 | NS142 | No direct equivalent | Titanium stabilised |
| 904L | N08904 | B673, B674, B677, B649 | 1.4539 | 015Cr21Ni26Mo5Cu2 | No direct equivalent | Not a standard A240 grade |
| Titanium Gr2 | R50400 | B265, B338, B348 | 3.7035 | TA2 | VT1-0 | Commercially pure, 40 ksi minimum yield |
Table note: cross-references per the current editions of the cited ASTM specifications and the corresponding EN, GB and GOST standards; grade equivalences are approximate and do not imply identical chemistry or nitric acid performance.
Titanium in Nitric Acid: Excellent Below the Fuming Range, Unacceptable Above It
Titanium Grade 2 is one of the best materials available for nitric acid containing chloride, and one of the worst for fuming nitric acid. In aerated nitric acid up to about 65% and up to roughly 100 °C, commercially pure titanium forms a stable TiO2 film and corrodes at rates well under 0.1 mm/y, while remaining immune to the chloride pitting and chloride stress corrosion cracking that limit every austenitic option. That combination is why titanium tubing is common in nitric acid condensers and coolers where the cooling water is brackish or where chloride ingress cannot be excluded.
The limits are concentration, temperature and water content, and they are sharper than most selection charts suggest. Above about 65-70% concentration the corrosion rate of titanium rises, and at boiling azeotropic strength it becomes unacceptable for continuous service. Above 98%, in fuming acid containing free NO2, titanium is not merely unsuitable but hazardous: the metal can react vigorously with anhydrous nitric acid and nitrogen tetroxide, and dry NOx systems have a history of titanium fires and energetic failures. Any titanium specification for nitric service must therefore state a minimum water content and a maximum NO2 content, and must exclude fuming acid and dry NOx by name. Titanium is also attacked by dilute acid in the complete absence of water, an unusual condition but one that appears in vapour-phase and anhydrous systems.
Fabrication adds two practical constraints. Titanium has low thermal conductivity and a strong affinity for oxygen, so welding requires inert gas shielding of the root and the hot trailing edge, and contamination shows up as a colour change from silver through straw to blue and violet. A blue or white weld in nitric service is a corrosion initiation site, not a cosmetic defect. Titanium also galls and has limited wear resistance, so tube-to-tubesheet joints, flanges and support contacts need design attention. Where these constraints are respected, titanium is often the lowest-lifecycle-cost answer for a chloride-contaminated nitric acid condenser, even at two to three times the tube cost of 310L.
| Acid concentration | Temperature | Titanium Gr2 corrosion rate, typical | Suitability | Comment |
|---|---|---|---|---|
| 10-30% | Ambient to 60 °C | Under 0.05 mm/y | Suitable | Chloride-bearing streams acceptable |
| 30-65% | 60-100 °C | 0.05-0.1 mm/y | Suitable | Standard condenser and cooler duty |
| 65-68% | 100-120 °C | 0.1-0.5 mm/y | Marginal, verify by test | Approaching the practical ceiling |
| 68-80% | Ambient to 60 °C | 0.1-0.3 mm/y | Marginal, typical | Water content must be controlled |
| Above 98% fuming, NO2 present | Any | Not applicable | Not suitable | Risk of vigorous reaction and ignition |
| Anhydrous NOx, dry vapour | Any | Not applicable | Not suitable | Exclude titanium by specification |
Table note: rates are typical values from ASTM G31 immersion-test literature and supplier corrosion data for commercially pure titanium per ASTM B265 / B338 (latest edition); actual rates depend on water content, aeration and surface condition.
Condensers, Reboilers and the Condensing Zone: Where Nitric Acid Is Most Aggressive
The condensing zone is the most aggressive location in a nitric acid plant, and a material selected for the bulk acid will often fail there. Three things happen at once on a condensing surface: the liquid film becomes more concentrated than the bulk vapour, non-condensable gases such as NO and oxygen change the local potential, and non-volatile chloride concentrates in the film as water and acid evaporate. A 304L tube that would last fifteen years in a 40% acid storage tank can perforate in two years in the first condensing pass of the same plant's condenser.
The concentration effect is straightforward. Nitric acid and water form an azeotrope at about 68%, and the vapour leaving a bleacher or a concentrator can be richer in acid than the liquid it came from. As that vapour condenses, the first droplets are the most concentrated and the most oxidising, and they wet the tube wall at the highest metal temperature in the exchanger. This is where 310L or a high-silicon grade earns its cost, and it is why the tube specification for a nitric acid condenser should state the composition of the first condensate rather than the average acid strength of the circuit.
Non-condensables matter more than most selection guides admit. NO2 and NO are always present to some degree in nitric acid vapour, and oxygen ingress through poor venting or through dissolved air in cooling water changes the cathodic reactions available at the surface. A condenser that is properly vented and runs with a small oxygen content behaves differently from one that accumulates inert gas and runs with a low oxygen partial pressure in the condensing zone. In the second case, the passive film on a lean grade becomes less stable and the corrosion rate climbs, which is one reason two identical condensers in the same plant can show very different tube lives.
Velocity and tube grade interact. In clean condensing service a moderate acid velocity is beneficial because it replenishes the ions needed to repair the passive film and prevents deposits from establishing a crevice. In a condenser with entrained solids, catalyst fines or precipitated salts, the same velocity erodes the film and produces under-deposit attack. Nitric acid condensers generally run at low liquid velocities in the tubes, which makes deposit control and tube cleaning access a design requirement rather than a maintenance afterthought. Where velocity has to be raised to control deposits, titanium is more tolerant than the austenitics because its film repairs faster and it does not pit in chloride.
| Exchanger duty | Typical acid condition | Tube grade | Shell or header grade | Velocity guidance | Key risk |
|---|---|---|---|---|---|
| Bleacher overhead condenser | 60-68%, 100-120 °C, NOx present | 310L | 310L or 304L NAG | 0.5-1.5 m/s | First-condensate concentration, intergranular attack |
| Concentrator condenser | Up to 68%, hot, chloride possible | 310L or high-silicon austenitic | 310L | 0.5-1.5 m/s | Chloride concentration in film |
| Dilute acid cooler | 20-50%, 40-80 °C | 304L NAG | 304L NAG | 1.0-2.0 m/s | Chloride pitting, cooling water leakage |
| Mixed acid cooler | HNO3 plus H2SO4, 40-90 °C | Alloy 20 or 825 | Alloy 20 or 825 | 1.0-2.0 m/s | Reducing acid character, erosion |
| Nitric acid condenser with brackish cooling water | 30-65%, up to 100 °C | Titanium Gr2 | 304L NAG or titanium | 1.0-2.5 m/s | Tube-side fouling, water-side chloride |
| Fuming acid cooler | Above 98%, NO2 present | Aluminium or high-silicon austenitic | Same as tubes | Low | NO2 reaction, ignition risk with titanium |
Table note: duty descriptions and velocity ranges are typical design practice; tube and shell grades should be confirmed against the applicable ASME VIII Div 1 design case, the stream analysis and the results of ASTM G31 immersion testing.
Welding, Fabrication, Cleaning and the QA Tests That Predict Service Life
Welding and cleaning decide the service life of nitric acid equipment more often than grade selection does, because both create the grain-boundary chemistry and surface contamination that the acid attacks. Three rules cover most of the risk: keep carbon and heat input low, keep molybdenum out of the weld unless the specification calls for it, and keep free iron off the surface. Everything else in a nitric acid fabrication specification is detail around those three.
Low-carbon practice means more than buying 304L. It means a maximum interpass temperature, typically 150 °C or below, controlled heat input, no preheat, and a welding procedure that has been qualified with corrosion testing rather than only with tensile and bend tests. For 304L NAG the filler is normally ER308L, matching the parent metal's chromium and nickel without adding molybdenum. A 316L filler, which is what a fabricator may reach for out of habit, deposits 2-3% molybdenum into a weld that will spend its life in strongly oxidising acid, and it also raises the ferrite level. Where the specification permits only austenitic weld metal, ER308L with a controlled ferrite number or a fully austenitic filler may be required, and the drawing must say which.
Ferrite is a genuine nitric acid issue rather than a theoretical one. Delta ferrite in a duplex weld microstructure is preferentially attacked in nitric acid, so a weld with 8-10 FN can show selective ferrite dissolution and a corrosion rate several times that of the parent plate in the Huey test. Many nitric acid specifications therefore cap ferrite, require a ferrite check on the weld, and in some cases require the weld metal itself to be Huey tested. The same logic applies to 310L, where matching ER310 filler is used and the high nickel content keeps the weld fully austenitic.
Cleaning is where Chinese fabrication shops most often lose a nitric acid order on site. Carbon steel tooling, wire brushes, grinding discs, slings and even the rollers of a plate bending machine transfer free iron to the stainless surface, and that iron rusts in nitric acid service within days, producing brown stains that a client reads as material failure. The remedies are well established: dedicated stainless tools, iron-free grinding consumables, pickling and passivation per ASTM A380, and a final ferroxyl or equivalent free-iron check on welds and heat-affected zones. Hydrotest water is part of the same discipline, because chlorinated or high-chloride water left in a vessel over a weekend can initiate pitting before the plant ever runs.
| Material | Filler for nitric service | Ferrite control | Interpass temperature | Post-weld treatment | Notes |
|---|---|---|---|---|---|
| 304L NAG | ER308L | 3-8 FN typical, capped by specification | 150 °C max | Pickle and passivate per ASTM A380 | No molybdenum-bearing filler unless specified |
| 310L / 310S | ER310 | Fully austenitic, typical | 150 °C max | Pickle and passivate per ASTM A380 | Higher heat input tolerance than 304L |
| High-silicon austenitic | Matching high-silicon filler | Fully austenitic | 100 °C max, typical | Pickle and passivate | Segregation-sensitive, qualified procedure essential |
| Alloy 20 | ER320LR | Fully austenitic | 150 °C max | Pickle and passivate | Low carbon, niobium-bearing |
| 825 | ERNiCrMo-3 or ERNiCr-3 | Not applicable | 150 °C max | Pickle and passivate | Nickel-base filler, dilution control |
| 904L | ER385 | Fully austenitic | 150 °C max | Pickle and passivate | Molybdenum-rich, avoid excessive dilution |
| Titanium Gr2 | ERTi-2 | Not applicable | 200 °C max, typical | Inert gas shielding, no pickling required | Colour check for oxygen contamination |
Table note: filler classifications per AWS A5.9 / A5.14 and consumable guidance in the cited ASTM product specifications; interpass temperatures and ferrite limits are typical fabrication practice, not standard requirements.
| Grade | Solution annealing range | Cooling | Stress relief | Forbidden range | Typical reason |
|---|---|---|---|---|---|
| 304L NAG | 1010-1120 °C | Water or rapid air | 400 °C max, or full anneal | 450-850 °C | Sensitisation and carbide precipitation |
| 310L / 310S | 1035-1120 °C | Water or rapid air | 400 °C max, or full anneal | 500-900 °C | Sigma and carbide formation |
| High-silicon austenitic | 1050-1100 °C, typical | Water quench | Not normally used | 500-900 °C | Sigma and silicide precipitation |
| Alloy 20 | 940-1010 °C | Water quench | 900 °C anneal preferred | 650-900 °C | Niobium carbide and sigma |
| 825 | 930-1030 °C | Rapid quench | 940 °C anneal preferred | 650-870 °C | Titanium carbide and sigma |
| 904L | 1090-1170 °C | Water quench | 400 °C max, or full anneal | 500-900 °C | Sigma formation |
| Titanium Gr2 | 700-800 °C, 1-3 h | Air cool | 480-650 °C | Above 850 °C | Grain growth and oxygen pickup |
Table note: annealing ranges are typical values consistent with ASTM A240 / A480, ASTM B463, ASTM B424, ASTM B673 and ASTM B265 (latest editions); actual parameters must come from the mill's qualified heat treatment procedure.
| Grade | Condition | Yield strength, min or typical | Tensile strength | Elongation | Temperature basis |
|---|---|---|---|---|---|
| 304L NAG | Solution annealed | 170 MPa min | 485 MPa min | 40% min | Room temperature, ASTM A240 |
| 304L NAG | Solution annealed | 105 MPa typical | 390 MPa typical | - | 400 °C, typical design data |
| 310S / 310L | Solution annealed | 205 MPa min | 515 MPa min | 40% min | Room temperature, ASTM A240 |
| 310S / 310L | Solution annealed | 130 MPa typical | 430 MPa typical | - | 600 °C, typical design data |
| Alloy 20 | Solution annealed | 240 MPa min | 550 MPa min | 30% min | Room temperature, ASTM B463 |
| Alloy 20 | Solution annealed | 165 MPa typical | 470 MPa typical | - | 400 °C, typical design data |
| 825 | Solution annealed | 240 MPa min | 550 MPa min | 30% min | Room temperature, ASTM B424 |
| 825 | Solution annealed | 160 MPa typical | 460 MPa typical | - | 540 °C, typical design data |
| 904L | Solution annealed | 220 MPa min | 490 MPa min | 35% min | Room temperature, ASTM B673 |
| Titanium Gr2 | Annealed | 275 MPa min | 345 MPa min | 20% min | Room temperature, ASTM B265 |
| Titanium Gr2 | Annealed | 190 MPa typical | 300 MPa typical | - | 300 °C, typical design data |
Table note: minimum values per the cited ASTM product specifications (latest editions) at room temperature; elevated-temperature values are typical design data for use with ASME VIII Div 1 allowable stress tables and must not be substituted for code values.
The QA plan for a nitric acid order should be built around the failure modes rather than around generic mill testing. The Huey test per ASTM A262 Practice C is the acceptance test for 304L NAG, high-silicon grades and welds in those grades; Practice E, the Strauss test, is the intergranular test normally applied to 316L, 904L and Alloy 20, where copper sulphate and sulphuric acid detect chromium depletion rather than the strongly oxidising attack of nitric acid; Practice A, the oxalic acid etch, is a fast screening test that flags sensitised heats before the slow tests are run. Positive material identification per ASTM E1476 closes the mix-up route, and a ferrite check on welds closes the fabrication route. A purchase order that names all four, plus a weld procedure qualification with corrosion testing, is what a nitric acid plant should be buying.
| Test | Standard | What it detects | Applied to | Acceptance typical |
|---|---|---|---|---|
| Oxalic acid etch | ASTM A262 Practice A | Sensitisation screening | 304L, 310L, 316L | Step structure, no ditches |
| Huey test | ASTM A262 Practice C | Intergranular attack in oxidising acid | 304L NAG, 310L, high-silicon, welds | Max 0.6 mm/y per period, typical |
| Strauss test | ASTM A262 Practice E | Chromium depletion at grain boundaries | 316L, 904L, Alloy 20 | No cracking on bend, typical |
| PMI | ASTM E1476 | Grade mix-up, alloy verification | All grades, all forms | Composition within specification |
| Ferrite check | ASTM A800 or equivalent | Delta ferrite in weld metal | 304L NAG, 310L welds | 3-8 FN, typical |
| Free iron check | ASTM A380 | Iron contamination | Finished surfaces, welds | No rust or blue discolouration |
| Weld procedure corrosion test | ASTM A262 Practice C on coupon | Weld and HAZ corrosion resistance | All nitric acid welds | Rate within parent metal limit |
Table note: test methods per ASTM A262 and ASTM A380 (latest editions); acceptance values are typical nitric acid plant requirements and must be written into the purchase order to be enforceable.
2026 Price Reference and Lead Times for Nitric Acid Alloys
Nitric acid alloy selection is usually cost-driven at the bottom of the range and risk-driven at the top, so the price gap between 304L NAG and the nickel alloys is worth stating plainly. Through 2026 nickel has traded well below its 2022 spike, which has compressed the premium on the nickel-rich grades and shortened mill lead times for 304L NAG and 310L; titanium sponge and titanium mill products have stayed firm because aerospace and chemical demand have both been strong. The practical effect is that the step from 304L NAG to 310L is cheap, the step to Alloy 20 or 825 is a real project cost, and the step to titanium is justified only by a chloride problem that cannot be solved otherwise.
The table below is indicative only. Alloy surcharges move with nickel, molybdenum, copper and titanium scrap, and Chinese export pricing also moves with the exchange rate and with domestic mill loading. Treat the numbers as a budget tool and ask for a firm offer against a stated specification, quantity and delivery window.
| Grade | Product form assumed | Indicative price range, USD/kg | Relative to 304L NAG | Typical lead time |
|---|---|---|---|---|
| 304L NAG | Plate, 6-20 mm | 3.6-4.6 | 1.0 | 4-6 weeks |
| 310L / 310S | Plate, 6-20 mm | 6.5-8.5 | 1.9 | 5-7 weeks |
| Alloy 20 | Plate, 6-20 mm | 13-17 | 3.8 | 8-12 weeks |
| 825 | Plate, 6-20 mm | 14-18 | 4.1 | 8-12 weeks |
| 904L | Plate, 6-20 mm | 11-15 | 3.3 | 6-10 weeks |
| Titanium Gr2 | Plate, 6-20 mm | 24-32 | 7.0 | 6-10 weeks |
Table note: indicative 2026, EXW Shanghai, USD/kg ranges for solution-annealed plate in the stated thickness; prices move with nickel, molybdenum and titanium scrap and with order quantity, and are not offers.
Standard Index
| Standard | Title or scope | Covers | Product form |
|---|---|---|---|
| ASTM A240 / A480 | Chromium and chromium-nickel stainless steel plate, sheet and strip; general requirements | 304L, 310S chemistry and mechanicals | Plate, sheet, strip |
| ASTM A312 | Seamless and welded austenitic stainless steel pipe | 304L, 310 pipe | Pipe |
| ASTM A213 | Seamless ferritic and austenitic alloy steel boiler and heat exchanger tubes | 304L, 310 tube | Tube |
| ASTM A262 | Detecting susceptibility to intergranular attack in austenitic stainless steels | Practices A, C and E | Test method |
| ASTM A380 | Cleaning, descaling and passivation of stainless steel parts | Pickling and passivation | Fabrication |
| ASTM B463 / B464 / B468 | UNS N08020 plate, sheet and strip; welded pipe; welded tube | Alloy 20 | Plate, pipe, tube |
| ASTM B423 / B424 / B425 | UNS N08825 pipe; plate, sheet and strip; bar | 825 | Pipe, plate, bar |
| ASTM B673 / B674 / B677 | UNS N08904 plate, sheet and strip; seamless tube; welded tube | 904L | Plate, tube |
| ASTM B265 / B338 | Titanium and titanium alloy strip, sheet and plate; seamless and welded tube | Titanium Gr2 | Plate, tube |
| ASTM E1476 | Metals identification, grade verification and sorting | PMI | Test method |
| ASME VIII Div 1 | Rules for construction of pressure vessels | Design and allowable stress | Equipment |
Table note: standard numbers and scopes per the latest editions of the cited ASTM and ASME documents; always purchase against the current edition and state it on the order.
FAQ: Nitric Acid Alloy Selection
Q1: What is the best alloy for nitric acid service?
There is no single best alloy, because nitric acid duty splits into three zones that need different materials. For dilute to 65% acid at ambient to moderate temperature, 304L nitric acid grade is the best answer on both corrosion resistance and cost, provided it passes the Huey test and the chloride level stays under about 50 ppm. For hot azeotropic acid around 65-68% at the boiling point, 310L is the standard choice, with high-silicon austenitic grades where 310L shows unacceptable metal loss. For fuming acid above 98%, aluminium or a high-silicon austenitic is required and 304L must not be used. Where chlorides or sulphuric acid are also present, Alloy 20, 825, 904L or titanium enter the picture. The correct process is to fix the concentration, the temperature, the chloride level and any mixed-acid component first, then select against the narrowest of those limits and confirm the choice with a corrosion test result rather than a datasheet.
Q2: Why does 304L nitric acid grade cost more than standard 304L?
Nitric acid grade 304L carries restricted carbon, silicon, phosphorus and sulphur, and it must pass the Huey test per ASTM A262 Practice C, so the mill has to use cleaner scrap, tighter melting control, different deoxidation practice and additional testing. Typical nitric acid grade limits are carbon 0.020% maximum, silicon 0.30% maximum, phosphorus 0.020% maximum and sulphur 0.005% maximum, all tighter than the ASTM A240 base values. The testing is a real cost: five 48-hour boiling periods per heat, with specimen preparation, solution renewal and certified results. The price premium is usually modest, in the range of a few percent to about ten percent over commodity 304L, and it buys a corrosion rate guarantee that the commodity grade does not carry. Buying commodity 304L and hoping for the best is the false economy that produces intergranular failures at welds two or three years into service, when a replacement vessel costs far more than the original upgrade.
Q3: Can I use 316L instead of 304L NAG for nitric acid?
You can, but you gain nothing and you lose intergranular margin. 316L carries 2-3% molybdenum, and molybdenum is not beneficial in strongly oxidising nitric acid; at high concentration and temperature it can slightly increase the corrosion rate. The molybdenum also raises the risk of sigma phase formation during welding and reduces the ferrite control options open to the fabricator. What 316L does not carry is the restricted silicon, phosphorus and sulphur that a nitric acid grade needs, so its Huey test result is usually worse and less predictable than a properly produced 304L NAG. The one situation where 316L makes sense is a nitric acid stream with a genuine chloride problem at moderate temperature, and even there 904L or 310L is usually the better answer. If a drawing specifies 316L for nitric acid, ask what the molybdenum is for; if the answer is chloride, replace it with a grade selected for chloride rather than accepting a compromise that satisfies neither requirement.
Q4: What is the Huey test and what acceptance value should I specify?
The Huey test is ASTM A262 Practice C: a specimen is boiled in 65% nitric acid for five consecutive 48-hour periods, with the solution renewed each period, and the mass loss is converted to a corrosion rate in millimetres or inches per year. It detects intergranular attack caused by chromium depletion and is the classical acceptance test for nitric acid grade stainless steel. Typical purchase requirements are a maximum of about 0.6 mm/y (0.024 in/y) in each period, with many nitric acid and adipic acid plants tightening the five-period average to about 0.36 mm/y (0.014 in/y). These are buyer requirements rather than values written into ASTM A262, so the purchase order must state the exact rule, the number of periods, whether the average or every period is judged, and whether a single failed period rejects the lot. Specify the test on the parent plate and on a production-representative weld procedure coupon, because the weld is where the rate usually rises.
Q5: Is 304L suitable for fuming nitric acid?
No. Fuming nitric acid, above about 98% concentration with free NO2 present, attacks austenitic stainless steels intergranularly and can produce metal loss rates above 1 mm/y in a single campaign, so 304L, 310L and even 904L are excluded from that service. The correct materials are aluminium 1060 for tanks and lines at ambient temperature, or a high-silicon austenitic grade where higher strength or better erosion resistance is needed. Fuming acid also requires strict attention to sealing and venting, because moisture ingress dilutes the acid locally and creates a dilute pocket that behaves completely differently from the bulk, and because NO2 is toxic and corrosive in its own right. If your process can drift into the fuming range during an upset, specify the material for the fuming case rather than for the normal operating point, and add a water-content limit to the operating envelope so that the assumption is visible to the next engineer who reviews the file.
Q6: How much chloride can 304L tolerate in nitric acid?
Roughly 50 ppm is the practical ceiling, and even that depends on temperature, velocity and crevice geometry. Nitric acid holds stainless steel at a high potential close to the pitting breakdown potential, so chloride pitting starts at much lower levels than in neutral water or dilute sulphuric acid. Above about 60 °C, 50-100 ppm chloride is enough to pit 304L and to trigger chloride stress corrosion cracking at welds, cold-worked bends and tube expansions. The trap is concentration: evaporators, reboilers and condensers concentrate non-volatile chloride in the liquid film, so a bulk analysis of 20 ppm can correspond to several hundred ppm at the tube wall. Sample the condensate and the first condensing zone, not only the bulk acid. If chloride cannot be excluded, step up to 310L for modest levels, 904L for a few hundred ppm at moderate temperature, Alloy 20 or 825 for mixed acid, or titanium where chloride is the dominant problem and the fuming range is excluded.
Q7: When should I choose Alloy 20 instead of 304L for nitric acid?
Choose Alloy 20 when the stream is a nitrating mixed acid, meaning nitric acid combined with a substantial sulphuric acid content, or when nitric acid carries chloride together with sulphuric acid. In that environment the acid behaves as a mixed reducing-oxidising system, and the molybdenum, copper and niobium in Alloy 20 (N08020) become beneficial rather than neutral. Typical nitration streams contain 15-30% nitric acid with 50-70% sulphuric acid, and Alloy 20 has been the standard material for nitrators, mixed acid feed lines and spent acid recovery for decades. Do not choose Alloy 20 for a pure nitric acid tank or fractionator: its Huey corrosion rate in boiling 65% nitric acid is typically higher than a good 304L NAG, and it costs roughly four times as much. The decision rule is simple: if the sulphuric acid content is significant, Alloy 20 or 825; if it is absent and the chloride is low, 304L NAG. Ask for a full spent-acid analysis, including chloride and fluoride, before committing to either grade.
Q8: Is titanium a good choice for nitric acid heat exchangers?
Titanium Grade 2 is an excellent choice for nitric acid condenser and cooler tubes up to about 65% concentration and roughly 100 °C, especially where the cooling water is brackish or chloride ingress cannot be excluded. Its TiO2 film is stable in aerated nitric acid, it corrodes at well under 0.1 mm/y in that range, and it is immune to the chloride pitting and chloride stress corrosion cracking that limit austenitic grades. The exclusions matter: titanium is not suitable above about 68-70% concentration at temperature, and it must never be used in fuming nitric acid or dry NOx service, where it can react vigorously. Fabrication also demands inert gas shielding on both sides of the weld and a colour check for oxygen contamination. Where those conditions are met, titanium often gives the lowest lifecycle cost in a chloride-contaminated condenser, even at two to three times the tube cost of 310L. Ask the tube mill for a corrosion test in the actual acid before committing to a full bundle.
Q9: Which filler metal should be used for welding 304L NAG?
ER308L is the normal filler for 304L nitric acid grade, matching the 19% chromium and 10% nickel of the parent metal without adding molybdenum. Do not substitute ER316L out of habit: it deposits 2-3% molybdenum into a weld that will live in strongly oxidising acid, and it changes the ferrite balance. Control interpass temperature to about 150 °C maximum, keep heat input moderate, and qualify the procedure with a corrosion test on a production-representative coupon rather than only with tensile and bend tests. Ferrite should be controlled, typically 3-8 FN, and checked on the actual weld, because delta ferrite is preferentially attacked in nitric acid. Where a fully austenitic weld is required, the drawing must say so and the filler must be selected accordingly. Finally, clean the weld and heat-affected zone per ASTM A380 and verify the absence of free iron before shipment, since a correct weld with a contaminated surface fails just as quickly as a wrong filler.
Q10: What is the difference between 310L and 904L for nitric acid?
310L is a high-chromium, high-nickel, molybdenum-free austenitic designed for hot oxidising service, and it is the correct upgrade from 304L when nitric acid temperature or concentration rises toward the azeotrope. Its 24-26% chromium holds the passive film in boiling 65% acid where 304L cannot. 904L is a chloride-resistant grade with 19-23% chromium, 4-5% molybdenum and 1.5% copper, designed for sulphuric acid and chloride-bearing streams; in hot concentrated nitric acid its molybdenum is not an advantage and it may corrode faster than 310L. The practical rule is that 310L answers a temperature problem and 904L answers a chloride problem. If both temperature and chloride are high, neither is ideal: Alloy 20, 825 or titanium becomes the candidate, and the choice should be confirmed with immersion testing in the actual stream rather than by comparing datasheets side by side.
Q11: How do I avoid free iron contamination on nitric acid equipment?
Assume every carbon steel surface in the fabrication shop is a contamination source and design the workflow around that assumption. Use dedicated stainless steel wire brushes, grinding discs, slings, clamps and marking tools; keep stainless plate off carbon steel racks; and cover the finished surfaces during blasting, painting and hydrotesting of adjacent carbon steel items. Pickle and passivate per ASTM A380 after fabrication, including weld heat tint removal, because heat tint is a chromium-depleted oxide that will corrode in nitric acid even when the underlying metal is correct. Finish with a free iron check, either the ferroxyl test or a controlled acid rinse, on welds and heat-affected zones. Specify the maximum chloride content of hydrotest water, typically below 30 ppm, and require draining and forced drying immediately after the test. These steps cost little and prevent the brown rust stains that make a client reject a vessel that is metallurgically sound.
Q12: What should a nitric acid alloy purchase order include?
A nitric acid purchase order should state the grade, the UNS number, the ASTM product specification and its edition, the nitric acid grade restrictions with actual values, the Huey test per ASTM A262 Practice C with the acceptance rule and whether each period or the average is judged, PMI per ASTM E1476, and the ferrite limit for welds. Add the filler metal, the welding procedure qualification requirement including corrosion testing of the coupon, cleaning and passivation per ASTM A380, and the free iron check. State the product form and dimensions against ASTM A240 / A480, A312 or A213 as applicable, and require the mill certificate to show measured rather than typical values. Finally, state the chloride limit of the hydrotest water. A purchase order that says only "304L, nitric acid grade" leaves the most important acceptance criterion undefined, and that is where most disputes between buyer and mill begin.
Conclusion: Select for the Stream, Then Prove It With a Test
The selection rule for nitric acid is short enough to put on a drawing: chromium content sets the concentration and temperature ceiling, molybdenum is a liability unless sulphuric acid or chloride is present, and the purchase specification is a corrosion rate rather than a chemistry table. 304L NAG covers dilute to 65% acid at moderate temperature and is the default for storage, piping and dilute coolers. 310L covers the azeotrope and hot acid. High-silicon austenitics and aluminium cover the concentrated and fuming range. Alloy 20 and 825 cover nitrating mixed acid. 904L covers moderate chloride, and titanium covers chloride-bearing condensers below the fuming range.
The second half of the rule is verification. A nitric acid plant that buys the right grade but skips the Huey test on the weld, or accepts a vessel with free iron on the heat-affected zone, will see failures that look like grade-selection errors and are not. Put ASTM A262 Practice C on the plate and on the weld procedure coupon, put ASTM A262 Practice E on the 904L and Alloy 20 items, put PMI and a ferrite check on every heat, and put ASTM A380 cleaning and a free iron check on the finished surface. Those four clauses cost less than one unplanned shutdown.
If you are selecting for a nitric acid or nitration circuit and want the grade and the test plan reviewed together, our engineers will compare your stream analysis against the concentration, temperature and chloride limits above. Browse our stainless steel plate, tube and bar range for 304L NAG and 310L, our Incoloy 825 and nickel alloy product range for mixed acid duty, and our titanium Grade 2 tube and plate range for chloride-bearing condensers, then send your duty conditions and drawing to our sales team for a firm offer with the test certificates included.
Related Reading
- The big three acids: selecting alloys for sulfuric, hydrochloric and phosphoric acid service in 2026
- Sulfuric acid alloy selection: round bar, seamless tube and plate supply from Shanghai
- Nickel alloy pickling and passivation: what ASTM A380 actually requires
Contact & Complete Product Range
Shanghai Hangbo Alloy Group Co., Ltd. - China Supplier
Email: sales@hangboalloy.com | WhatsApp (Lisa): +86 13611656360 | www.nickel-alloy.com
All Grades
Ni: NI200-N6 | Monel: 400-502, K-500, R-405 | Inconel: 600-740H, X-750, 725 | Incoloy: 800-27-7MO | Hastelloy: C-276-HYBRID-BC1, N | Super Austenitic: 904L-AL-6XN | Chromium-Rich: Alloy 33 | High-Strength Stainless: Nitronic 50/60, PH13-8Mo | Chlorination: Alloy 45 | Nimonic: 75-263 | Haynes: 25-HR-160 | RA: 330/333 | Precision: 1J22-4J45 | High-Strength: 18Ni250-AerMet100 | Heating: Cr20Ni80/60 | Specialty: Alloy 20-602CA
Product Forms: Bars(6-500mm) | Tubes(OD 6-610mm) | Plates(0.1-100mm) | Forgings | Welded Pipes | Fittings | Wire(0.05-10mm) | Strip(0.02-4.0mm)