Pulp and Paper Alloy Selection: Digester to Bleach Plant (56 chars)
Date: 2026年10月27日 Categories: News Views: 410
By Shanghai Hangbo Alloy Group Co., Ltd. - China Supplier | ISO 9001:2015 | Est. 2012
Contact: sales@hangboalloy.com | hangbo@nickel-alloy.com | WhatsApp (Lisa): +86 13611656360
Quick Answer: which alloy for which pulp mill zone?
There is no single pulp mill alloy. Use 316L where chlorides stay low and temperatures stay moderate, 2304 or 2205 where caustic or chloride SCC risk rises above roughly 60 °C, 904L and 6Mo (AL-6XN) for chlorination and chlorine dioxide filtrates, Alloy 20 for mixed acid, and titanium Gr2/Gr7 only in oxidising, wet chloride service.
Key Takeaways
- Caustic SCC in white liquor is a residual-stress problem first and a corrosion-rate problem second: at 50-60 °C and above, a stressed 316L weld can crack in liquor that removes less than 0.05 mm/yr from an unstressed coupon.
- Chlorination stage filtrate (pH 1-2, chloride 500-3,000 mg/L, dissolved chlorine) is outside 316L's pitting range; 904L and the 6Mo grades are the working alloys there.
- 2205 duplex handles chlorine dioxide filtrate at low and moderate temperature; its practical ceiling is roughly 150-175 °C, after which 6Mo or a nickel alloy takes over.
- Crevice attack under gaskets, scale and biofilm is the leading bleach-plant failure mode, and it is solved by drainage and joint design as much as by grade.
- Duplex welds must hold a ferrite-austenite balance near 50/50 with nitrogen-bearing shielding gas; an unbalanced, nitrogen-starved root corrodes first in bleach filtrate.
- Buy on certificate and PMI, not on "equivalent" wording: duplex needs Mo and N verified, plus ASTM A923 and ASTM G48 evidence.
Why a Mill-Wide Material Map Beats a Single-Grade Datasheet
A kraft mill is not one corrosive service. It is a chain of services that differ by a factor of ten in chloride content, a factor of thirty in pH and up to 80 °C in temperature, often within a hundred metres of pipe rack. Alloy selection therefore starts from the flowsheet, not from a preferred grade list. A 316L that gives fifteen years in a neutral brown stock vat can perforate in two years in the chlorination stage downstream, and a duplex that survives bleach filtrate indefinitely will erode away in a blow line if the velocity is left uncapped.
The commercial consequence is that pulp and paper alloy selection is rarely about finding the most corrosion-resistant metal. It is about spending money in the two or three zones where the mechanism actually bites, and refusing to spend it in the eight zones where 316L is genuinely adequate. Mills that upgrade everything to 904L usually discover afterwards that they still have erosion in the knotters and crevice attack under the same old gaskets.
Four failure mechanisms that look alike in a failure report
Caustic stress corrosion cracking, chloride pitting, crevice corrosion and erosion-corrosion all present as localised metal loss or cracking, and all four get misdiagnosed as "bad material" in the first meeting. They are separated by three variables: temperature, chloride activity and stress. Caustic SCC needs concentrated hydroxide, a tensile stress at or near yield and roughly 50-60 °C; it does not need chloride at all. Chloride pitting needs an oxidising potential and a chloride activity above the grade's resistance, which is why chlorination stage filtrate destroys 316L but leaves 904L intact. Crevice corrosion needs a geometry that lets chloride concentrate while oxygen is starved. Erosion-corrosion needs velocity and, in slurries, particle hardness.
The map below is the working summary used for line-by-line material take-offs. It is deliberately organised by zone rather than by alloy, because that is the order in which the P&ID is reviewed.
| Zone | Dominant mechanism | Controlling variables (typical) | Alloys that hold | Common misapplication |
|---|---|---|---|---|
| White liquor storage, digester shell and circulation | Caustic SCC, erosion-corrosion | 20-35% NaOH equivalent, 120-170 °C, residual stress near yield | Stress-relieved 316L, 2304, 2205, 904L for high-chloride liquor | Unstress-relieved 316L welds and cold-formed bends |
| Digester blow line and knotters | Erosion-corrosion, flashing slurry | 3-8 m/s stock velocity, 100-140 °C, sand and shive load | 2205, 6Mo for high-velocity elbows | 316L at uncapped velocity or tight elbows |
| Brown stock washing and screening | Pitting, crevice under deposits | pH 6-11, chloride 100-800 mg/L, 60-90 °C | 316L, 2304 where chloride drifts up | 316L with stagnant drains and poor slope |
| Chlorination stage (C stage) | Oxidising chloride pitting, crevice | pH 1-2, chloride 500-3,000 mg/L, 40-60 °C | 904L, AL-6XN, Alloy 20 | 316L washers and repulper dilution laterals |
| Chlorine dioxide stages (D0, D1, D2) | Chloride SCC, pitting | pH 2-5, chloride 200-1,500 mg/L, 50-85 °C | 2205 low temperature, 6Mo above 70-80 °C | 316L in D0 filtrate heaters and seal water |
| Tall oil and turpentine recovery | Organic acid attack, SCC in hot vapour | 100-180 °C, naphthenic and resin acids, sulphur | 316L, 904L, Alloy 20 for acid condensate | Carbon steel in turpentine condenser necks |
| Recovery boiler lower furnace and smelt spouts | Sulphidation, molten smelt corrosion | 250-400 °C metal, Na2S/NaOH smelt | Composite tubes (304L/SA210), Alloy 625 overlays | Solid 316L in smelt contact zones |
Table note: mechanism assignments and temperature windows summarised from NACE SP0403 (latest edition) caustic SCC guidance, ASTM G48 (latest edition) test practice and published mill experience; all temperatures and concentrations are typical operating values, not specification limits.
Where the money actually goes
In a typical bleached kraft line, the digester and the bleach plant together account for most of the alloy spend, but for opposite reasons. The digester is a low-chloride, high-temperature, high-stress environment where the answer is often a properly stress-relieved 316L or a duplex, and the cost driver is fabrication discipline rather than alloy content. The bleach plant is a high-chloride, low-pH, moderate-temperature environment where the answer is genuinely a higher-alloy metal, and the cost driver is the price of molybdenum and nickel.
That split matters when budgets are cut. Removing stress relief from digester internals saves a few percent of fabrication cost and creates a cracking liability that appears in three to seven years. Substituting 316L for 904L in a chlorination stage washer saves perhaps 55-60% of the material cost and creates a perforation that appears in eighteen months.
White Liquor and the Digester: Caustic SCC Is a Stress Problem
White liquor does not crack stainless steel because it is corrosive. It cracks it because it is a hot hydroxide solution in contact with metal that is already carrying a tensile stress close to its yield point. The corrosion rate of annealed 316L in white liquor at 150 °C is low, typically below 0.05 mm/yr; a weld with 300 MPa of residual stress in the same liquor can crack through wall in a few thousand hours. Treating caustic SCC as a corrosion-rate problem leads to thicker walls, which change nothing, instead of to stress relief, which changes everything.
The three conditions that must coincide are well established in NACE SP0403 (latest edition) for carbon steel and apply in modified form to austenitic stainless: hydroxide concentration above roughly 5% (white liquor runs 20-35% NaOH equivalent, with Na2S and Na2CO3 present), metal temperature above roughly 50-60 °C, and tensile stress at or above the yield strength. Remove any one and cracking stops. In a digester at 150-170 °C the first two are fixed by the process, so stress is the only variable the designer controls.
Where the residual stress comes from
Three sources dominate, and all three are fabrication decisions rather than metallurgical ones. First, weld shrinkage: a 12 mm butt weld in a restrained nozzle or a shell seam develops transverse residual stress approaching the yield strength of the weld metal, and duplex weld metal yields higher than the parent. Second, cold forming: bends formed at 15-20% outer-fibre strain retain a through-wall stress gradient that survives service for decades, and a cold-formed elbow is the single most common caustic SCC initiation site in digester circulation piping. Third, fit-up and assembly stress: pulled joints, tack-welded misalignment and unrelieved nozzle loads add a sustained applied stress on top of the residual field.
The practical hierarchy is straightforward. Where geometry permits, solution-anneal the finished component at 1040-1120 °C and water-quench, which removes the residual field entirely. Where the component is too large to anneal, control the stress instead: weld sequence balanced around the neutral axis, back-step welding, no cold bends tighter than 1.5D, no forming strain above 10%, and full-penetration welds with smooth caps to remove stress raisers. Low-temperature "stress relief" at 400-450 °C, often requested by buyers who are used to carbon steel practice, does essentially nothing for austenitic stainless and should be rejected during technical review.
| Parameter | 316L (S31603) | 2304 (S32304) | 2205 (S32205) | 904L (N08904) |
|---|---|---|---|---|
| Solution anneal temperature, °C | 1040-1120 | 1000-1060 | 1020-1100 | 1090-1170 |
| Cooling after anneal | Water quench or rapid air | Water quench | Water quench | Water quench |
| Post-weld heat treatment for caustic service | Full solution anneal preferred; low-temperature relief ineffective | Not used; full anneal if required | Not used; full anneal if required | Full solution anneal |
| Maximum cold-forming strain before re-anneal, % (typical) | 10-15 | 10 | 10 | 10-15 |
| Minimum bend radius, cold, typical | 1.5D | 1.5D | 1.5D | 1.5D |
| Interpass temperature limit, °C | 150 | 150 | 150 | 150 |
Table note: annealing ranges per ASTM A240/A480 (latest edition) and ASTM A789/A790 (latest edition) for the duplex grades; the cold-forming and interpass limits are typical shop-floor practice, not standard requirements.
What this means for grade choice in the digester
Where liquor chloride is controlled below a few hundred mg/L and the component can be stress-relieved, 316L remains a defensible choice for digester shells, flash tanks and liquor heaters, and it is still the most common liner material in continuous digesters. Where chloride climbs above roughly 500-1,000 mg/L, usually through salt in the makeup white liquor or through carryover of bleach plant filtrate into the brown stock system, pitting adds to the SCC risk and 2304 or 2205 becomes the better trade: both resist caustic SCC to higher temperature, both have roughly twice the yield strength of 316L, and 2205's pitting resistance equivalent is high enough to ignore chloride levels that pit 316L.
The counter-argument is welding. Duplex in a digester requires the fabrication controls described later in this article, and a mill without a qualified duplex procedure is better served by stress-relieved 316L than by a duplex weld it cannot control. Digester internals also see erosion from chip and liquor circulation, which favours the higher hardness of duplex regardless of corrosion considerations.
Brown Stock Washing: Chlorides and Acidity Set the 316L Boundary
Brown stock washing sits between two aggressive zones and is often wrongly treated as benign. The liquor starts alkaline at pH 10-12 on the last wash stage and drifts toward pH 6-7 as fresh water and acidic carryover mix, while temperature stays at 60-90 °C and chloride accumulates from wood, from mill water and from bleach plant filtrate reused to the washers. Under those conditions 316L performs well in the bulk liquid and fails at the edges: under gasket faces, beneath fibre mats on the vat floor, at the vapour space of the seal tank, and wherever a drain line holds stagnant liquor.
The chloride threshold is the number to establish first. Below roughly 200-300 mg/L at 70 °C, 316L gives long life with normal maintenance. Between 300 and 800 mg/L, pitting appears under deposits and at crevices while the general corrosion rate stays low, and 2304 or 2205 is the economical upgrade because it buys pitting resistance without the cost of a nickel-base alloy. Above roughly 1,000 mg/L with any oxidant present, only the 6Mo class and above hold reliably, and at that point the mill should also be looking at where the chloride is coming from.
Why the seal tank vapour space fails first
The seal tank and the washer hood combine three aggravating factors: a wet-dry cycling surface, chloride concentration by evaporation at the waterline, and biological activity that produces both sulphide and acid. Stainless that is fully immersed and wetted is protected; stainless that cycles wet and dry accumulates chloride salts that deliquesce into a concentrated film. The corrosion potential under that film can exceed the pitting potential of 316L even when the bulk liquor is harmless. Vapour-space corrosion is therefore a geometry and ventilation problem, and the fix is a slope, a drain and a demister rather than a thicker plate.
Where the vapour space cannot be kept dry, a 2205 or 904L hood is worth the premium; both tolerate chloride salt films far better than 316L, and 904L's copper addition gives it useful resistance in the mixed acidic condensate that forms where chlorine dioxide vapours condense.
Chlorination Stage: Oxidising Chloride at Low pH
The chlorination stage is the most aggressive continuous environment in a bleached kraft mill, and it is aggressive for a reason that 316L cannot answer: it combines low pH, high chloride and a strong oxidant. C-stage filtrate typically runs pH 1-2 with 500-3,000 mg/L chloride at 40-60 °C, and the dissolved chlorine raises the corrosion potential well above the pitting potential of any 300-series stainless. The result is not general wastage but deep, undercut pits that initiate at inclusions and at weld oxides and penetrate at rates that make wall-thickness allowances meaningless.
The relevant property is the critical pitting temperature measured by ASTM G150 (latest edition) in chloride solution, or the pitting resistance equivalent number calculated as Cr + 3.3Mo + 16N. Neither is a design guarantee, but both rank the candidate alloys correctly. For 316L the CPT in 1 M NaCl is typically 20-25 °C, which is below the operating temperature of every C-stage washer; for 904L it is typically 45-55 °C; for AL-6XN it is typically 65-75 °C. That single comparison explains why 316L C-stage washers fail in months, why 904L survives in the C stage but can struggle in a hot D0 filtrate heater, and why the 6Mo grades exist at all.
| Alloy | UNS | Standard | Cr, % | Ni, % | Mo, % | Cu, % | N, % | C, max % | PREn, typical |
|---|---|---|---|---|---|---|---|---|---|
| 316L | S31603 | ASTM A240 / A480 | 16.0-18.0 | 10.0-14.0 | 2.00-3.00 | — | 0.10 max | 0.030 | 25 |
| 2304 | S32304 | ASTM A240 / A789 / A790 | 21.5-24.5 | 3.0-5.5 | 0.05-0.60 | 0.50 max | 0.05-0.20 | 0.030 | 26 |
| 2205 | S32205 | ASTM A240 / A789 / A790 / A928 | 22.0-23.0 | 4.5-6.5 | 3.0-3.5 | — | 0.14-0.20 | 0.030 | 35 |
| 904L | N08904 | ASTM B673 / B674 / B677 | 19.0-23.0 | 23.0-28.0 | 4.0-5.0 | 1.0-2.0 | 0.10 max | 0.020 | 36 |
| AL-6XN | N08367 | ASTM B688 / B691 / B675 | 20.0-22.0 | 23.5-25.5 | 6.0-7.0 | 0.75 max | 0.18-0.25 | 0.030 | 46 |
| Alloy 20 | N08020 | ASTM B463 / B464 / B468 | 19.0-21.0 | 32.0-38.0 | 2.0-3.0 | 3.0-4.0 | — | 0.07 | not applicable |
| Ti Gr2 | R50400 | ASTM B265 / B338 | — | — | — | — | 0.03 max (N) | 0.08 | not applicable |
| Ti Gr7 | R52400 | ASTM B265 / B338 | — | — | — | — | 0.03 max (N) | 0.08 | not applicable |
Table note: composition limits per ASTM A240/A480 (latest edition) for S31603, S32304 and S32205, ASTM B673 (latest edition) for N08904, ASTM B688 (latest edition) for N08367, ASTM B463 (latest edition) for N08020 and ASTM B265 (latest edition) for titanium; PREn is a calculated ranking value, not a specification requirement. Ti Gr7 contains 0.12-0.25% Pd; Ti Gr2 oxygen maximum is 0.25%.
Where titanium wins and where it does not
Titanium Gr2 is the default for chlorination tower internals, ClO2 mixer nozzles, washer drums and seal water piping because it is immune to chloride pitting and crevice corrosion in wet oxidising chloride at any temperature a bleach plant can produce. That immunity is conditional. Titanium is attacked by dry chlorine gas, and titanium in anhydrous or high-velocity dry chlorine can ignite; the metal depends on a water film to maintain its oxide. It also picks up hydrogen in low-pH, low-potential crevices and becomes brittle, which is why Gr7 with 0.12-0.25% palladium is specified for tight crevices and for upset conditions where the potential can fall.
Titanium is also a poor choice for high-velocity slurry and for sliding contact, because it galling and it erodes readily; and it is not a general answer to chlorine dioxide. In ClO2 stages titanium has given excellent service in washers and in the D1/D2 filtrate system, but failures have been reported where dry chlorine dioxide vapour contacts titanium in the absence of moisture, and in vapour spaces where chloride salts concentrate and the potential shifts. The rule used in most mills is: titanium for wet oxidising chloride, never for dry chlorine, and Gr7 rather than Gr2 wherever a gasket crevice or a stagnant drain cannot be eliminated.
Alloy 20 in the mixed-acid corners
Alloy 20 (N08020) is not a bleach plant bulk material, but it earns its place in the small items where sulphuric acid meets chloride: acid cleaning connections, sulphamic acid dosing, tall oil acidulation piping and the acid stage of some specialist pulps. Its 3-4% copper and niobium-stabilised chemistry give it resistance to sulphuric acid that no duplex has, while its 32-38% nickel keeps it immune to chloride SCC at bleach plant temperatures. It is a poor choice for oxidising chloride because it lacks the molybdenum and nitrogen to resist pitting, which is precisely why it is not specified for C-stage washers.
Chlorine Dioxide Bleaching: The Classic Chloride SCC Environment
Chlorine dioxide stages are where pulp mill alloy selection is most often decided by temperature rather than by chemistry, because the chemistry is only moderately aggressive while the temperature is not. D0 filtrate runs pH 2-4 with 200-1,500 mg/L chloride at 50-85 °C; the D1 and D2 stages are hotter and cleaner, sometimes reaching 85-90 °C in a pressurised stage. There is no free chlorine to speak of, but the chloride is there, the pH is low, and the metal is welded, which is the full set of conditions for chloride SCC in austenitic stainless.
This is the environment that made 2205 duplex the standard bleach plant material in the 1990s and 2000s, and the reason is mechanical rather than electrochemical. Duplex resists chloride SCC because its ferrite phase breaks up the continuous austenite path a crack needs; it resists pitting because 3% molybdenum and 0.17% nitrogen give it a PREn of about 35. But duplex is a two-phase alloy with a temperature ceiling, and above roughly 150-175 °C the ferrite phase becomes the weak link in chloride SCC and the alloy loses its advantage over 316L. That ceiling is not a sharp line, and it moves with stress, oxygen and chloride level.
| Service condition | Temperature, typical | Chloride, typical | First choice | Why |
|---|---|---|---|---|
| D2 stage, low chloride, low temperature | 60-70 °C | 200-500 mg/L | 2205 | Duplex SCC resistance with pitting margin |
| D1 stage, moderate chloride | 70-80 °C | 500-1,000 mg/L | 2205 or 904L | Duplex where stress is controlled; 904L where chloride drifts |
| D0 stage, high chloride, hot | 80-90 °C | 1,000-1,500 mg/L | AL-6XN or 904L | 6Mo CPT margin above operating temperature |
| D0 filtrate heater, pressurised | 100-140 °C | 500-1,500 mg/L | AL-6XN, Alloy C-276 for tube side | Above duplex SCC ceiling |
| Chlorination stage washer | 40-60 °C | 500-3,000 mg/L | 904L, AL-6XN, Ti Gr2 drum | Oxidising chloride, low pH |
| ClO2 generator and chlorine dioxide vapour | 40-80 °C | high, plus ClO2 gas | Ti Gr2/Gr7, 6Mo for wet vapour | Titanium immune when wet, attacked when dry |
Table note: temperature and chloride bands are typical operating ranges compiled from bleach plant practice; the duplex temperature ceiling of roughly 150-175 °C is a typical engineering limit, not a standard limit, and must be confirmed against ASME B31.3 (latest edition) allowable stresses for the specific grade at design temperature.
Why the duplex ceiling exists and how to respect it
The 475 °C embrittlement that limits duplex at high temperature is a separate phenomenon from the SCC ceiling, and neither is a reason to avoid duplex below 150 °C. What matters in bleach plant design is that the ceiling is reached earlier when three conditions stack: high chloride, high residual stress and an oxidising potential. A 2205 D0 filtrate line at 85 °C with chloride at 1,200 mg/L and a poorly fitted flange is a different risk from the same line at 60 °C with 400 mg/L. Where the stack is unavoidable, the answer is a 6Mo grade or 904L, not a thicker duplex wall.
The economics are clear enough: 2205 costs roughly 60-70% of 904L per kilogram and about 40% of AL-6XN, so specifying duplex across the whole bleach plant and upgrading only the hot, high-chloride nodes is normally the lowest-cost compliant design. That is exactly the pattern this material map is meant to produce.
Crevice Corrosion Under Gaskets, Deposits and Biofilms
If you tabulate bleach plant failures by cause rather than by alloy, crevice corrosion leads. The mechanism is simple: a shielded geometry lets oxygen be consumed faster than it can be replenished, chloride migrates in to balance the charge, pH inside the crevice falls to 1-3, and the metal inside becomes an anode while the bold surface becomes a large cathode. The result is a narrow, deep attack that perforates a 3 mm washer shell in a season while the adjacent wetted surface looks new.
Three crevice types account for most of the damage. Gasket faces on flanges, manways and instrument connections are the first; the crevice is created by the gasket itself and is often aggravated by a gasket that is too wide, over-torqued or made of a material that degrades and leaves a porous residue. Deposits are the second: fibre mats on washer vat floors, lime and scale in seal water lines, and pulp stock that settles in low points during shutdowns. Biofilms are the third and the least recognised; a sessile bacterial film on stainless in a warm chloride environment creates an oxygen-depleted, acidic pocket directly on the surface, and it does so on vertical walls where no one expects a crevice.
| Gasket / joint material | Temperature limit, typical | Chlorination stage | ClO2 stage | Comment |
|---|---|---|---|---|
| PTFE envelope with EPDM core | 120 °C | Good | Good | Preferred general bleach plant gasket; low chloride leach |
| Virgin PTFE, full | 150 °C | Good | Good | Cold flow; requires retaining ring |
| Glass-filled PTFE | 150 °C | Good | Fair | Filler can leach in hot oxidising acid |
| Graphite laminate | 400 °C | Not recommended | Not recommended | Galvanic couple and chloride retention in wet oxidant |
| FKM (Viton) | 200 °C | Fair | Poor | Swells and degrades in ClO2; residue creates crevice |
| Compressed fibre / aramid | 150 °C | Poor | Poor | Wicks liquor, leaves fibre mat, worst crevice generator |
Table note: temperature limits and chemical ratings are typical values from gasket manufacturers' published data and mill experience; they are not standard requirements and must be confirmed for the specific joint design and torque procedure.
Design rules that actually remove crevices
Drainage is the highest-value fix and the cheapest. Every horizontal run in a bleach filtrate system should slope to a low point with a full-bore drain, every washer vat floor should fall to a sump, and every shutdown procedure should include a flush with low-chloride water before the line sits idle. A line that drains has no crevice at the bottom; a line that holds 40 mm of stagnant filtrate for three weeks has a crevice for its whole length.
Joint design is the second. Use the narrowest gasket that seals, never a full-face gasket on a raised-face flange, and specify a filled PTFE envelope rather than a compressed fibre sheet. Weld all internal joints full penetration and grind flush; a partial-penetration weld in a bleach filtrate line is a crevice with a crack starter attached. Where a crevice is unavoidable, upgrade the local material to a 6Mo grade or titanium Gr7, or apply a weld overlay, rather than upgrading the whole component.
Flushing and monitoring complete the picture. A monthly low-chloride flush of stagnant branches, a chloride analysis on seal water, and a shutdown inspection that opens the same three flanges every year will find crevice attack before it perforates. The inspection should target the downstream side of gaskets and the six o'clock position of horizontal runs, which is where the attack always is.
Erosion-Corrosion in Circulation, Blow Lines and Knotters
Digester circulation, blow lines, knotters and screened rejects lines fail by a different mechanism again: flowing liquor removes the passive film faster than it can reform, and the bare metal underneath corrodes at a rate set by velocity, temperature and, where sand or shive load is present, particle impact. The damage signature is a horseshoe-shaped wear pattern downstream of a weld, a thinning at the extrados of an elbow, or a grooved impeller eye. Corrosion rate alone predicts none of it.
Velocity therefore becomes a design parameter with a number attached. For clean white liquor at 120-160 °C, 316L is normally limited to about 1.5-2.5 m/s in continuous service, 2304 and 2205 to about 3-4 m/s, and the 6Mo grades to about 4-5.5 m/s. These are typical engineering limits used for line sizing, not standard values, and they tighten as sand, grit or shive content rises. For stock at 3-8% consistency, the limits fall by roughly 30-40% because the fibre mat scours the surface, and the elbows become the controlling items.
| Alloy | Hardness, typical | Max velocity, clean liquor (m/s, typical) | Max velocity, stock 3-8% (m/s, typical) | Relative erosion resistance |
|---|---|---|---|---|
| 316L | 140-160 HB | 1.5-2.5 | 1.0-1.8 | 1.0 (reference) |
| 2304 | 200-230 HB | 3.0-3.5 | 2.0-2.5 | 2.0 |
| 2205 | 240-270 HB | 3.5-4.5 | 2.2-3.0 | 2.5 |
| 904L | 140-170 HB | 2.0-3.0 | 1.3-2.0 | 1.1 |
| AL-6XN | 160-190 HB | 4.0-5.5 | 2.5-3.5 | 2.2 |
| Alloy 20 | 150-180 HB | 2.0-2.8 | 1.3-1.9 | 1.1 |
| Ti Gr2 | 150-180 HV | 3.0-5.0 | 1.5-2.5 | 0.8 |
Table note: hardness and velocity limits are typical values from mill practice and published erosion-corrosion guidance; they are not standard limits. Confirm line sizing against the owner's piping specification and ASME B31.3 (latest edition) velocity and wall-thickness rules.
Designing the high-velocity nodes
The useful discipline is to separate the line into bulk sections, where corrosion resistance governs, and nodes, where erosion governs. Bulk digester circulation piping in 2205 with a velocity cap of 4 m/s will outlast the same line in 316L by a wide margin, but the two elbows after the circulation pump should be specified separately: either a larger radius, a thicker schedule, a 6Mo grade, or a cast hard-facing alloy. Knotter and screen internals, blow line elbows and the discharge of high-consistency pumps are node items.
Two further points are often missed. First, velocity limits apply to the actual bore, so a line designed for 3 m/s and later operated at 5 m/s because a pump was uprated will erode; the material selection file should record the velocity limit alongside the grade. Second, erosion-corrosion is temperature-sensitive, and the 20 °C rise between a cold mill and a tropical summer can move a marginal line into rapid wastage. Where a blow line is already at its velocity limit, reducing flow or increasing bore is more effective than any alloy change at the same bore.
For slurry and high-solids service, the erosion mechanism is dominated by particle hardness and impact angle rather than by the alloy's corrosion resistance, and the appropriate grades are covered in the erosion-corrosion guide linked at the end of this article.
Tall Oil, Turpentine and the Recovery Boiler
The fourth zone fails for reasons that have nothing to do with chloride, and it is usually left out of alloy reviews until a condenser neck perforates. Crude tall oil comes out of black liquor soap acidulation, where sulphuric acid at 90-100 °C meets residual caustic and chloride; turpentine comes off the digester relief condenser as a hot vapour loaded with sulphur compounds; and the recovery boiler lower furnace runs a reducing atmosphere in contact with molten smelt at 250-400 °C metal temperature. Three different chemistries, three different answers.
Tall oil acidulation and the crude tall oil storage and transfer system are the classic Alloy 20 application in a pulp mill. The 3-4% copper and niobium-stabilised grade resists dilute sulphuric acid at temperature and is immune to chloride SCC, and it outperforms both 316L and the duplex grades in the acidulation reactor and the soap acidulation piping. Where the acid strength is low and the temperature moderate, 316L is often adequate; where the crude tall oil is hot and the acid concentration fluctuates, 904L is a defensible middle option, though it is weaker than Alloy 20 in sulphuric acid.
Tall oil distillation is a different problem: 200-280 °C under vacuum with fatty and resin acids, where the controlling damage is high-temperature organic acid attack plus erosion at the column internals. 316L is the baseline, 904L is used for the hotter trays and the pitch bottoms, and the real limit is mechanical rather than chemical, because no austenitic stainless has useful strength above about 550 °C.
Turpentine service is best handled by 316L for the decanter and by 316L or 904L for the condenser, with the caution that the vapour space accumulates sulphur and organic deposits that create crevices. The recovery boiler is a separate discipline: lower furnace walls are composite co-extruded tubes with a 304L outer layer over a carbon steel pressure tube, smelt spouts and smelt dissolving tank agitators carry nickel-base overlays such as Alloy 625, and solid stainless has no place in direct smelt contact. Specifying 316L plate for a smelt spout because it is "the stainless we have" is a recurring and expensive error.
Welding Duplex: Ferrite-Austenite Balance Decides the Life
Duplex earns its bleach plant position only if the weld matches the parent metal, and that is a fabrication problem, not a purchasing one. A 2205 weld that cools too fast, or that is shielded without nitrogen, ends up with the wrong phase balance and a root that pits in bleach filtrate years before the parent plate shows anything. The failure is always at the weld, always on the root side, and always in the grade that was bought specifically to avoid pitting.
The target is a ferrite content of roughly 35-65% in the weld metal and the heat-affected zone, with 40-60% being the usual working range for 2205 in pulp mill service. Ferrite number should be measured on the production weld, not inferred from the filler certificate, using a calibrated ferrite scope and the procedure qualification record. Too much ferrite gives poor toughness and preferential attack of the ferrite in some acids; too little gives a continuous austenite path and loses the SCC resistance that justified duplex in the first place.
Nitrogen is the controlling variable. Duplex filler metals contain 0.10-0.20% nitrogen for 2205, and the root purge must not strip it: argon alone gives a lean, nitrogen-depleted root, so a 2-3% nitrogen addition to the purge gas, or a nitrogen-bearing shielding gas for the root pass, is standard practice for bleach plant pipe. Heat input must stay in the 0.5-1.5 kJ/mm band for 2205, interpass temperature below 150 °C, and stringer beads rather than wide weave. No post-weld heat treatment: duplex held above about 300 °C precipitates sigma and loses both toughness and corrosion resistance, so any specification calling for PWHT on duplex should be rejected at review.
| Parameter | 2304 | 2205 | 6Mo (AL-6XN) | Comment |
|---|---|---|---|---|
| Ferrite in weld, target % | 40-65 | 35-65 (40-60 working) | 35-60 | Measure with calibrated ferrite scope |
| Heat input, kJ/mm, typical | 0.5-1.6 | 0.5-1.5 | 0.5-1.2 | Higher input coarsens and balances ferrite |
| Interpass temperature, °C max | 150 | 150 | 150 | Thermocouple on the joint, not the shop floor |
| Root purge oxygen, ppm max | 50 | 50 | 50 | Below 100 ppm for corrosion-critical root |
| Purge nitrogen addition, % | 2-3 | 2-3 | 2-3 | Protects nitrogen in the root |
| Post-weld heat treatment | None | None | None | Sigma phase above roughly 300 °C |
| Root cleaning | Pickle and passivate | Pickle and passivate | Pickle and passivate | Remove heat tint before hydrotest |
Table note: ranges are typical qualified-procedure values for gas tungsten arc and gas metal arc welding of duplex and super-austenitic grades; the ferrite targets follow ASTM A923 (latest edition) practice and filler metal manufacturers' recommendations, and the final values must come from the project's procedure qualification record.
Why the weld root is the first thing to go
A bleach filtrate line gives the root of a gusseted weld three things at once: a crevice formed by the gusset, a heat-tint oxide that is cathodic to the parent, and a nitrogen-depleted, ferrite-skewed microstructure. Under those conditions the root can pit at a chloride level that the parent metal tolerates by a factor of five. The repair is never a weld repair in situ; it is a redesign that removes the gusset and a re-qualified procedure that controls purge and heat input.
Two shop-floor controls close most of the gap. First, no open root without a purge dam and a measured oxygen reading, recorded per joint. Second, pickling and passivation of every duplex and 6Mo weld in bleach plant service, with the heat tint removed to a uniform grey before hydrotest. A wire brush is not pickling, and a heat tint left in place under a gasket is the most predictable corrosion initiation site in the plant.
QA and Purchasing: What to Verify Before the Plate Ships
The purchasing failure mode in pulp mill alloys is not usually a wrong grade; it is a right grade with the wrong paperwork, or a "904L equivalent" from stock that turns out to be 316L with a reprinted mill certificate. The three defences are product analysis, independent positive material identification, and grade-specific acceptance tests that a stockholder cannot fake.
Positive material identification to ASTM E1476 (latest edition) is the first line, and it must be done on the actual delivered item, not accepted from the mill certificate. For duplex the critical elements are molybdenum and nitrogen: a 2205 that reads 2.8% Mo and 0.12% N has the composition of a 31803 at best and will not deliver the pitting resistance the design assumed. Portable X-ray fluorescence measures molybdenum but cannot measure nitrogen or carbon, so duplex PMI must be paired with either a mill certificate showing nitrogen by inert gas fusion or a laboratory combustion check on a sample per heat.
| Alloy | Condition | Yield strength, MPa min | Tensile strength, MPa min | Elongation, % min | Yield at 200 °C, MPa typical | Tensile at 200 °C, MPa typical |
|---|---|---|---|---|---|---|
| 316L | Solution annealed | 170 | 485 | 40 | 130 | 420 |
| 2304 | Solution annealed | 400 | 600 | 25 | 320 | 520 |
| 2205 | Solution annealed | 450 | 620 | 25 | 350 | 540 |
| 904L | Solution annealed | 220 | 490 | 35 | 165 | 420 |
| AL-6XN | Solution annealed | 310 | 690 | 30 | 250 | 590 |
| Alloy 20 | Solution annealed | 240 | 550 | 30 | 190 | 480 |
| Ti Gr2 | Annealed | 275 | 345 | 20 | 200 | 300 |
Table note: room-temperature minimum values per ASTM A240/A480 (latest edition) for S31603, S32304 and S32205, ASTM B673 (latest edition) for N08904, ASTM B688 (latest edition) for N08367, ASTM B463 (latest edition) for N08020 and ASTM B265 (latest edition) for Ti Gr2, all in the solution-annealed condition; 200 °C values are typical and are given for preliminary sizing only, since design shall use the allowable stress values in ASME B31.3 (latest edition) at the design temperature.
The tests that separate a real duplex from a reprint
ASTM A923 (latest edition) is the duplex acceptance standard that matters, and it has three methods: metallographic examination for detrimental intermetallic phase, a Charpy impact test after ageing, and a ferric chloride corrosion test. A mill certificate that does not reference A923 for a bleach plant duplex order is incomplete, and a supplier who cannot explain which method was applied has not done the test. ASTM G48 Method A (latest edition) gives the pitting test in ferric chloride at a specified temperature and is the practical way to demonstrate that a 6Mo heat actually performs like a 6Mo; a 24-hour exposure at 50 °C with no weight loss and no visible pitting is the usual acceptance criterion for N08367 plate.
For 904L the trap is different. Because 904L is often bought as "904L equivalent" from stock, the certificate may show a chemistry range rather than a heat analysis, and the nickel may sit at the bottom of the 23-28% band while the molybdenum sits at 4.0%. That is still within ASTM B673 (latest edition), but it is a materially weaker alloy than a heat at 26% Ni and 4.8% Mo, and in a D-stage filtrate heater the difference shows up as pitting within two or three campaigns. The purchasing answer is to specify the heat analysis, require the actual values on the certificate, and reject certificates that quote only the specification range.
| Property | 316L | 2304 | 2205 | 904L | AL-6XN | Alloy 20 |
|---|---|---|---|---|---|---|
| PREN, typical | 25 | 26 | 35 | 36 | 46 | not applicable |
| CPT by ASTM G150, °C typical | 20-25 | 25-30 | 45-55 | 45-55 | 65-75 | 25-30 |
| Critical crevice temperature, °C typical | below 0 | 0-10 | 20-30 | 25-35 | 45-55 | 10-20 |
| Chloride SCC resistance | Poor above 60 °C | Good to 150 °C | Good to 150-175 °C | Good to 200 °C+ | Good to 200 °C+ | Good to 200 °C+ |
| Relative material cost index | 1.0 | 1.3 | 1.7 | 3.3 | 5.0 | 4.0 |
Table note: PREN calculated from the typical composition in the composition table above; critical pitting and crevice temperatures are typical values published for these grades in chloride media and are not standard guarantees; cost index is indicative and moves with nickel and molybdenum prices.
The 2026 buying context
Through 2026 the molybdenum-bearing grades have stayed on a wide price band, and the spread between 2205 and AL-6XN has widened enough that mills are re-examining where 6Mo is genuinely required. Nickel-based filler metal and 6Mo plate lead times from Chinese mills have been running four to eight weeks for standard sizes and longer for wide plate, while 316L and 2205 remain essentially ex-stock. That changes the optimisation: it is now usually cheaper to design the bleach plant around 2205 with 6Mo confined to the hot nodes than to standardise on a single high-alloy grade, and it is worth booking the 6Mo items early rather than substituting on the shop floor.
| Alloy | Product form | Indicative price, 2026, EXW Shanghai, USD/kg |
|---|---|---|
| 316L | Plate, 6-20 mm | 4.2-5.6 |
| 2304 | Plate, 6-20 mm | 5.0-6.5 |
| 2205 | Plate, 6-20 mm | 6.8-8.6 |
| 904L | Plate, 6-20 mm | 11.5-14.5 |
| AL-6XN (N08367) | Plate, 6-20 mm | 16-21 |
| Alloy 20 (N08020) | Plate, 6-20 mm | 14-18 |
| Ti Gr2 | Plate, 6-20 mm | 22-30 |
Table note: 2026, EXW Shanghai, USD/kg, indicative range only; prices move with nickel, molybdenum and titanium sponge, and are not a quotation. Confirm against a current offer for the specific heat, size and certification package.
Standard Index
| Standard | Title or scope | Covers | Product form |
|---|---|---|---|
| ASTM A240 / A480 | Chromium and chromium-nickel stainless steel plate, sheet and strip for pressure vessels; general requirements | 316L, 2304, 2205 chemistry and mechanical properties | Plate, sheet, strip |
| ASTM A789 | Seamless and welded ferritic/austenitic stainless steel tubing for general service | Duplex tube | Tube |
| ASTM A790 | Seamless and welded ferritic/austenitic stainless steel pipe | Duplex pipe | Pipe |
| ASTM A928 | Ferritic/austenitic steel pipe, electric-fusion-welded with filler metal | Duplex welded pipe | Welded pipe |
| ASTM A923 | Detecting detrimental intermetallic phase in duplex stainless steel | Microstructure, impact toughness, corrosion test | Wrought product, weld |
| ASTM B688 | Chromium-nickel-molybdenum-iron plate, sheet and strip (N08367) | AL-6XN flat product | Plate, sheet, strip |
| ASTM B691 | Welded pipe of N08367 | AL-6XN welded pipe | Welded pipe |
| ASTM B675 | Seamless pipe and tube of N08367 | AL-6XN seamless | Pipe, tube |
| ASTM B673 | Plate, sheet and strip of N08904, N08925, N08926 | 904L flat product | Plate, sheet, strip |
| ASTM B674 | Bar and forging stock of N08904, N08925, N08926 | 904L bar | Bar, forging stock |
| ASTM B677 | Seamless pipe and tube of N08904, N08925, N08926 | 904L seamless | Pipe, tube |
| ASTM B463 | Plate, sheet and strip of N08020 | Alloy 20 flat product | Plate, sheet, strip |
| ASTM B464 | Welded pipe of N08020 | Alloy 20 welded pipe | Welded pipe |
| ASTM B468 | Seamless and welded tube of N08020 | Alloy 20 tube | Tube |
| ASTM B265 | Titanium and titanium alloy strip, sheet and plate | Ti Gr2, Ti Gr7 | Plate, sheet, strip |
| ASTM B338 | Seamless and welded titanium and titanium alloy tubes for condensers and heat exchangers | Ti Gr2, Ti Gr7 tube | Tube |
| ASTM G48 | Pitting and crevice corrosion resistance of stainless steels and related alloys by ferric chloride | Pitting (Method A), crevice (Method B) | Coupon test |
| ASTM G150 | Electrochemical critical pitting temperature testing of stainless steels | CPT determination | Coupon test |
| ASTM E1476 | Guide for metals identification, verification and traceability | PMI practice | All forms |
| ASME B31.3 | Process piping | Allowable stress, wall thickness, velocity review | Pipe, fittings |
| NACE SP0403 | Avoiding caustic stress corrosion cracking of carbon steel | Caustic SCC conditions and stress relief | Equipment, piping |
Table note: standard numbers and scopes as published; always work to the latest edition and to the project specification, which may add requirements beyond the ASTM or ASME text.
FAQ: pulp and paper alloy selection
Q1: What alloy should I use for a kraft digester white liquor line?
Start with the chloride level and the stress state, not with a grade name. If liquor chloride stays below a few hundred mg/L and the spool can be fully solution-annealed, 316L is still a defensible choice at 120-160 °C, provided cold forming is limited and welds are smooth and full penetration. Once chloride climbs above roughly 500 mg/L, usually through salt in the makeup liquor or bleach filtrate carryover into the brown stock system, 2205 duplex is the better trade: it resists caustic SCC to a higher temperature, its pitting resistance equivalent of about 35 ignores chloride levels that pit 316L, and its yield strength is roughly 2.5 times higher. 2304 is a lower-cost duplex option where chloride and temperature are moderate. Where the line cannot be stress-relieved and the liquor is hot, choose duplex rather than thicker 316L, because caustic SCC is driven by stress, not by wall thickness. Ask for the heat analysis and confirm molybdenum and nitrogen before release.
Q2: Why does 316L crack in white liquor when the corrosion rate is low?
Because caustic SCC is a stress-corrosion mechanism, not a wastage mechanism. Three conditions must coincide: hydroxide concentration above roughly 5% (white liquor is 20-35% NaOH equivalent), metal temperature above roughly 50-60 °C, and a tensile stress at or near the yield strength. Under those conditions a crack initiates at a weld toe, a cold-formed bend or a fit-up stress raiser and propagates through wall in a few thousand hours, while an unstressed coupon in the same liquor loses less than 0.05 mm/yr. That is why thickness surveys and corrosion coupons come back clean while the line fails, and why adding corrosion allowance does nothing. The three practical controls are full solution annealing at 1040-1120 °C, cold-forming limits of about 10% strain before re-annealing, and weld sequencing that balances shrinkage. Low-temperature stress relief at 400-450 °C, which works for carbon steel, does not relieve residual stress in austenitic stainless and should not be accepted as a substitute.
Q3: Is 2205 duplex suitable for the chlorination stage?
No, not as the default material for a C-stage washer or repulper. Chlorination filtrate combines pH 1-2, chloride at 500-3,000 mg/L and dissolved chlorine, which raises the corrosion potential far above the pitting resistance of a 3% molybdenum duplex. The critical pitting temperature of 2205 in chloride solution is typically 45-55 °C, and C-stage liquor runs at 40-60 °C, so the margin is thin to negative, particularly under gaskets and deposits where the critical crevice temperature, typically 20-30 °C, is already exceeded. Duplex also suffers in very low pH oxidising chloride because the ferrite phase can be attacked selectively. The working alloys in the chlorination stage are 904L, AL-6XN and Alloy 20, with titanium Gr2 or Gr7 for tower internals and washer drums. Where a mill has standardised on 2205 for the bleach plant, the C stage must be carved out as an exception rather than designed by default. A duplex C-stage repulper that has run for two years without visible attack is not evidence that the grade is suitable, because pitting in this service is usually hidden under the stock mat and discovered only at the next wall-thickness survey.
Q4: What is the difference between 904L and AL-6XN for bleach plant service?
Both are austenitic, both resist chloride SCC to well above bleach plant temperatures, and both are specified in D-stage service. The difference is pitting and crevice margin. 904L (N08904) has about 20% chromium, 4-5% molybdenum and 1-2% copper, giving a pitting resistance equivalent near 36 and a critical pitting temperature typically 45-55 °C. AL-6XN (N08367) has 20-22% chromium, 6-7% molybdenum and 0.18-0.25% nitrogen, giving a PREn near 46 and a CPT typically 65-75 °C, with a critical crevice temperature around 45-55 °C against 25-35 °C for 904L. In practice AL-6XN is chosen where chloride exceeds roughly 1,000 mg/L, where the temperature exceeds 70-80 °C, or where crevices cannot be eliminated; 904L is chosen where the duty is moderate and cost matters. AL-6XN costs roughly 40-50% more per kilogram, so the decision should be made node by node rather than plant-wide, and the copper in 904L gives it an edge in the mixed acidic condensate that forms where ClO2 vapours condense on a cool hood surface.
Q5: Can I use titanium Gr2 in a chlorine dioxide stage?
Yes for wet service, with conditions. Titanium Gr2 is immune to chloride pitting and crevice corrosion in wet oxidising chloride at any bleach plant temperature, which is why it is standard for ClO2 mixer nozzles, washer drums, seal water piping and tower internals. The immunity depends on a water film maintaining the oxide, so dry chlorine gas is excluded: titanium can be attacked and can ignite in dry chlorine. Dry chlorine dioxide vapour in the absence of moisture is also a risk, and vapour spaces where chloride salts concentrate and the potential shifts have produced titanium failures. Where a gasket crevice or a stagnant drain cannot be eliminated, specify Gr7 with 0.12-0.25% palladium rather than Gr2, because the palladium lowers the corrosion potential and reduces hydrogen pickup that embrittles the metal in low-pH, low-potential pockets. Titanium is also poor in high-velocity slurry and in sliding contact, so do not use it for stock lines or knotters.
Q6: What causes pitting under gaskets in bleach plant washers?
Crevice corrosion, and it is the leading bleach plant failure mode. Inside a gasket, deposit or biofilm, oxygen is consumed faster than it can be replenished, chloride migrates in to balance the charge, and the pH falls to 1-3. The shielded area becomes a small anode coupled to a large cathodic bold surface, so attack is fast and deep: a 3 mm shell can perforate in a season while the adjacent wetted surface looks untouched. The control measures are geometric and procedural rather than metallurgical. Slope every horizontal filtrate run to a drain, flush stagnant branches with low-chloride water before shutdowns, use the narrowest gasket that seals, avoid compressed fibre sheet that wicks liquor, weld internal joints full penetration and grind flush, and inspect the six o'clock position of horizontal runs and the downstream side of gaskets every shutdown. Where a crevice is unavoidable, upgrade locally to a 6Mo grade or titanium Gr7 rather than the whole component.
Q7: What velocity limit should I use for 316L and duplex in digester circulation?
Use a velocity cap alongside every grade specification, because erosion-corrosion, not general corrosion, decides life in circulation and blow lines. For clean white liquor at 120-160 °C, a typical working limit for 316L is 1.5-2.5 m/s, for 2304 about 3-3.5 m/s, for 2205 about 3.5-4.5 m/s, and for the 6Mo grades 4-5.5 m/s. For stock at 3-8% consistency, reduce those figures by roughly 30-40%, because the fibre mat scours the surface and the elbows become the controlling items. These are typical engineering limits used for line sizing, not standard values, and they tighten as sand, grit or shive load rises. Two practical rules follow. Record the velocity limit in the material selection file so that a later pump uprate does not silently exceed it, and treat elbows, knotters, screen internals and blow line bends as separate node items with a larger radius, heavier schedule or higher grade, rather than upgrading the whole line. Where a line is already marginal, increasing the bore lowers the velocity far more cheaply than changing grade at the same bore.
Q8: Do duplex welds need post-weld heat treatment?
No. Duplex grades must not be post-weld heat treated, and a specification requiring PWHT on 2205 or 2304 should be rejected at technical review. Holding duplex above roughly 300 °C precipitates sigma and other intermetallic phases, which reduce toughness and corrosion resistance, and the damage is not recoverable by a subsequent anneal on a finished fabrication. The correct thermal treatment is a full solution anneal at 1020-1100 °C with water quenching, applied to the mill product or to a component that can be fully re-annealed, never as a local field treatment. What duplex welds do need is process control during welding: heat input in the 0.5-1.5 kJ/mm band, interpass temperature below 150 °C, stringer beads, a nitrogen-bearing purge of 2-3% for the root, and pickling and passivation to remove heat tint. Those controls, not PWHT, are what preserve the ferrite-austenite balance and the corrosion resistance that justified the grade.
Q9: How do I verify that a 2205 plate is really 2205?
Three checks, in order. First, positive material identification to ASTM E1476 (latest edition) on the delivered item, not a certificate review, confirming chromium, nickel and molybdenum. Second, a nitrogen value from the mill certificate by inert gas fusion, because portable XRF cannot measure nitrogen and nitrogen is half of what makes 2205 a duplex: a plate reading 2.8% Mo and 0.12% N is not S32205. Third, grade-specific acceptance evidence: ASTM A923 (latest edition) results covering microstructure, impact toughness and the ferric chloride corrosion test, plus a ferrite count on the production weld. Ask for the heat number to link the plate, the certificate and the test report. Where the order is for bleach plant service, add ASTM G48 Method A (latest edition) at a specified temperature as a performance check. A supplier who can produce all three without being chased is a supplier worth keeping; one who offers only a certificate with specification ranges has not verified anything.
Q10: Is "904L equivalent" acceptable for a bleach plant order?
Treat "equivalent" as a warning word, not a grade. 904L is defined by UNS N08904 and ASTM B673/B674/B677 (latest edition), with nickel at 23-28% and molybdenum at 4.0-5.0%. A heat at 23.5% Ni and 4.1% Mo and a heat at 27% Ni and 4.9% Mo both comply, but they are not the same alloy in a hot D-stage filtrate: the leaner heat has less austenite stability, a lower pitting resistance equivalent and a measurably lower critical pitting temperature. Stock sold as "904L equivalent" often carries a certificate quoting only specification ranges, sometimes from a remelt with no traceable heat number, and occasionally turns out to be 316L with reprinted paperwork. The purchasing answer is to specify UNS N08904, require the actual heat analysis values on the certificate, require PMI to ASTM E1476 on delivery, and require the ASTM G48 result if the duty is chlorination or hot ClO2. If the price is materially below the market range in this article, the metallurgy is probably not what the label says.
Q11: Which gasket material should I use in chlorination and ClO2 service?
Use a PTFE envelope gasket with an EPDM core as the default, and a virgin PTFE gasket with a retaining ring where the temperature runs above about 120 °C. Both resist chlorination and chlorine dioxide filtrate, do not wick liquor, and leave a clean flange face on disassembly. Avoid three common choices. Compressed fibre and aramid sheet wick liquor into the joint, leave a fibre mat behind and create the worst crevice in the plant. Graphite laminate is wrong in wet oxidising chloride because it couples galvanically and retains chloride. FKM (Viton) swells and degrades in chlorine dioxide, and the degraded residue forms a porous crevice that holds acidic filtrate against the flange face. Beyond material, control the geometry: use the narrowest gasket that seals, never a full-face gasket on a raised-face flange, torque to the gasket manufacturer's value rather than by feel, and replace gaskets at every shutdown rather than reusing a compressed joint.
Q12: How do I choose between 2304 and 2205 for brown stock washing?
Choose on chloride level, temperature and the presence of crevices. 2304 (S32304) has about 23% chromium, 4% nickel, 0.3% molybdenum and 0.1% nitrogen, giving a pitting resistance equivalent near 26, only marginally above 316L, but with roughly twice the yield strength and far better chloride SCC resistance. It suits brown stock washers, vat floors, hoods and stock lines where chloride stays in the 200-500 mg/L band at 60-80 °C and where the duty is more about strength and SCC than about pitting. 2205, with 3% molybdenum and 0.17% nitrogen and a PREn near 35, is the right choice once chloride exceeds roughly 500-800 mg/L, once deposits and gaskets create crevices, or once the liquor carries bleach plant filtrate. The price difference is roughly 25-30% per kilogram, which is small against a washer rebuild. Where the choice is genuinely marginal, take 2205 for anything downstream of a filtrate reuse connection.
Conclusion: Map the zones, then spend the money where the mechanism is
Pulp and paper alloy selection is a zoning exercise. Four zones fail for four different reasons: white liquor and the digester by caustic SCC driven by residual stress, brown stock washing by pitting and crevice attack as chloride and acidity fluctuate, chlorination and chlorine dioxide bleaching by oxidising chloride at low pH with a temperature ceiling that duplex cannot cross, and tall oil, turpentine and the recovery boiler by hot organic acids and smelt sulphidation. A single grade cannot answer all four, and a mill that tries usually ends up with a high-alloy plant that still cracks at the welds and erodes at the elbows.
The working rule is short. Use 316L where chloride is low, temperature is moderate and the fabrication can be stress-relieved. Move to 2304 or 2205 when chloride, temperature or stress rises, and accept duplex only with a qualified welding procedure and a nitrogen-bearing purge. Use 904L and 6Mo for the chlorination stage and the hot, high-chloride ClO2 nodes, Alloy 20 for acidulation and mixed acid, and titanium Gr2/Gr7 for wet oxidising chloride components within its dry-chlorine limits. Then verify: PMI on every duplex item, nitrogen from the certificate, ASTM A923 and ASTM G48 evidence, and gaskets and drainage treated as part of the material system.
For the product side, the stainless steel product range covers 316L, 2304, 2205, 904L and AL-6XN in plate, sheet, bar, seamless tube and welded pipe, the titanium product range covers Gr2 and Gr7 to ASTM B265 and B338, and the nickel alloy product range covers the C-family grades and Alloy 20 for the acidulation and recovery areas. Send the flowsheet zone, chloride level, temperature and product form through the contact page and the material can be quoted against the specific duty rather than against a generic grade list.
Related Reading
- Preventing chloride stress corrosion cracking in chemical heat exchangers: why 6Mo alloys such as 926 and SMO 254 are essential
- Chloride SCC failure analysis: what round bar, seamless tube and plate failures reveal about grade selection
- Nickel alloy erosion-corrosion in slurry service: velocity limits, hardness and grade selection
Contact & Complete Product Range
Shanghai Hangbo Alloy Group Co., Ltd. - China Supplier
Email: sales@hangboalloy.com | WhatsApp (Lisa): +86 13611656360 | www.nickel-alloy.com
All Grades
Ni: NI200-N6 | Monel: 400-502, K-500, R-405 | Inconel: 600-740H, X-750, 725 | Incoloy: 800-27-7MO | Hastelloy: C-276-HYBRID-BC1, N | Super Austenitic: 904L-AL-6XN | Chromium-Rich: Alloy 33 | High-Strength Stainless: Nitronic 50/60, PH13-8Mo | Chlorination: Alloy 45 | Nimonic: 75-263 | Haynes: 25-HR-160 | RA: 330/333 | Precision: 1J22-4J45 | High-Strength: 18Ni250-AerMet100 | Heating: Cr20Ni80/60 | Specialty: Alloy 20-602CA
Product Forms: Bars(6-500mm) | Tubes(OD 6-610mm) | Plates(0.1-100mm) | Forgings | Welded Pipes | Fittings | Wire(0.05-10mm) | Strip(0.02-4.0mm)